Jump to content

Specific Process Knowledge/Lithography/Resist/UVresist: Difference between revisions

From LabAdviser
Jehem (talk | contribs)
Jehem (talk | contribs)
Line 539: Line 539:


===Aligner: Maskless 02===
===Aligner: Maskless 02===
<!-- The Aligner: Maskless 02 has a 375 nm laser light source, and a 405 nm laser light source, each with a FWHM of ~1 nm. -->
The Aligner: Maskless 02 has a 375 nm laser light source with a FWHM of ~1 nm. All exposures on this tool are made using the optical autofocus system, unless otherwise specified.
The Aligner: Maskless 02 has a 375 nm laser light source with a FWHM of ~1 nm.


'''New resists'''<br>
'''Quality control'''<br>
As of 2023-03-21 we no longer have any of the old versions of the resists: AZ 5214E, AZ 4562, AZ MiR 701. The following table contains only information about the new resist versions.
Please note that the values listed in the table are <i>'''not'''</i> routinely tested as part of quality control, except for the resist AZ 5214E.
 
'''New writehead'''<br>
As of 2023-03-21 the MLA2 has a new writehead installed, converting it from a write mode 1 tool to a write mode 2 tool. This makes all previous dose/defocus settings obsolete. The following table contains only the dose/defocus values for the new writehead.
 
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"
|-


{| class="wikitable"
|-
|-
|-style="background:silver; color:black"
!  !! Date !! Operator !! Film thickness !! Exposure mode !! Dose !! Defoc !! Resolution !! Comments
|
!Date
!Thickness
!Laser
!Autofocus
!Exposure mode
!Dose
!Defoc
!Resolution
!Comments
|-
|-
 
! scope=row| AZ MIR 701
| 2023-08-21 || taran || 1.5 µm || Quality || 325 mJ/cm<sup>2</sup> || 1 || 1 µm || '''Not under regular quality control'''<br><br>Post exposure bake: 60 s @ 110°C<br>Development: 60 s puddle<br><br>Tested using dehydration reducing measures
|-
|-
|-style="background:WhiteSmoke; color:black"
! scope=row| AZ 5214E
!rowspan="2"| AZ MiR 701
| 2024-12-09 || taran || 1.5 µm || Quality|| 100 mJ/cm<sup>2</sup> || 2 || 1.5 µm || See QC data for latest values<br><br>Development: 60 s puddle
|rowspan="2"| 2023-08-21 <br> taran
|rowspan="2"| 1.5 µm
|rowspan="2"| 375
| Optical
|rowspan="2"| Quality
|rowspan="2"| 325 mJ/cm<sup>2</sup>
| 1
|rowspan="2"| 1 µm<br>Tested using dehydration reducing measures<br>(design elongated +40mm in y).
|rowspan="2"|
PEB: 60s @ 110°C<br>
Dev: SP60s
|-style="background:WhiteSmoke; color:black"
| Pneumatic
| ?
|-
|-
 
! scope=row| AZ 5214E<br>Image reversal
| 2023-04-17 || jehem || 2.2 µm || Quality|| 35 mJ/cm<sup>2</sup> || 0 || 1.5 µm || '''Not under regular quality control'''<br><br>Reversal bake: 60 s @ 110°C<br>Flood exposure: 500 mJ/cm<sup>2</sup><br>Development: 60 s puddle
|-
|-
|-style="background:silver; color:black"
! scope=row| AZ nLOF 2020  
!rowspan="2"| AZ nLOF 2020
| 2023-08-21 || taran || 2.0 µm || Quality || 450 mJ/cm<sup>2</sup> || 0 || 1.5 µm || '''Not under regular quality control'''<br><br>Post exposure bake: 60 s @ 110°C<br>Development: 60 s puddle
|rowspan="2"| 2023-08-21 <br> taran
|rowspan="2"| 2.0 µm
|rowspan="2"| 375
| Optical
|rowspan="2"| Quality
|rowspan="2"| 450 mJ/cm<sup>2</sup>
| 0
|rowspan="2"| 1.5 µm
|rowspan="2"|
PEB: 60s @ 110°C<br>
Dev: SP60s
|-style="background:silver; color:black"
| Pneumatic
| ?
|-
|-
! scope=row| AZ 4562
| 2023-04-19 || jehem || 10 µm || Quality|| 1150 mJ/cm<sup>2</sup> || 0 || ≤5 µm || '''Not under regular quality control'''<br><br>Priming: HMDS<BR>Rehydration after SB: none<br>Exposure: Single exposure<br>Degassing after exposure: none<br>Development: 5 x 60 s multi puddle
|}


|-
'''New writehead'''<br>
|-style="background:WhiteSmoke; color:black"
As of 2023-03-21 the MLA2 has a new writehead installed, converting it from a write mode 1 tool to a write mode 2 tool. This makes all previous dose/defocus settings obsolete. This table contains only the dose/defocus values for the new writehead.
!rowspan="2"| AZ 5214E
|rowspan="2"| 2024-12-09<br>taran
|rowspan="2"| 1.25 µm
|rowspan="2"| 375
| Optical
|rowspan="2"| Quality
|rowspan="2"| 100 mJ/cm<sup>2</sup>
| 2
|rowspan="2"| 1.5 µm
|rowspan="2"| Dev: SP60s<br>See QC data for latest values
|-style="background:WhiteSmoke; color:black"
| Pneumatic
| -2 (?)
|-
 
|-
|-style="background:silver; color:black"
!rowspan="2"| AZ 5214E<br>image reversal
|rowspan="2"| 2023-04-17 <br> jehem
|rowspan="2"| 2.2 µm
|rowspan="2"| 375
| Optical
|rowspan="2"| Quality
|rowspan="2"| 35 mJ/cm<sup>2</sup>
| 0
|rowspan="2"| 1.5 µm
|rowspan="2"|
Reversal bake: 60s @ 110°C<br>
Flood exposure: 500 mJ/cm<sup>2</sup><br>
Dev: SP60s
|-style="background:silver; color:black"
| Pneumatic
| ?
|-


|-
'''New resists version in 2023'''<br>
|-style="background:whitesmoke; color:black"
As of 2023-03-21 we no longer have any of the old versions of the resists: AZ 5214E, AZ 4562, AZ MiR 701. This table contains only information about the new resist versions.
!rowspan="2"| AZ 4562
|rowspan="2"| 2023-04-19<br>jehem
|rowspan="2"| 10 µm
|rowspan="2"| 375
| Optical
|rowspan="2"| Quality
|rowspan="2"| 1150 mJ/cm<sup>2</sup>
| 0
|rowspan="2"| ≤5 µm
|rowspan="2"|
Priming: HMDS<br>
Rehydration after softbake: 1 hour (may not be necessary)<br>
Exposure: Single exposure<br>
Degassing after exposure: 1 hour (may not be necessary)<br>
Development: Multiple puddles, 5 x 60 s
|-style="background:whitesmoke; color:black"
| Pneumatic
| ?
|-


|}
<br>
'''Dehydration reducing measures used for testing AZ MiR 701:'''<br>
'''Dehydration reducing measures used for testing AZ MiR 701:'''<br>
The CDA used for the pneumatic autofocus will dehydrate the resist. To reduce this effect, the writehead is parked far away from the write area while setting up the job for at least a few minutes, before starting the exposure.
The CDA used for the pneumatic autofocus will dehydrate the resist. To reduce this effect, the writehead is parked far away from the write area while setting up the job for at least a few minutes, before starting the exposure.
Line 669: Line 575:
<br clear="all" />
<br clear="all" />


New table
===Aligner: Maskless 03===
===Aligner: Maskless 03===
The Aligner: Maskless 03 has a 405 nm laser light source with a FWHM of ~1 nm. All exposures on this tool are made using the pneumatic autofocus system.
The Aligner: Maskless 03 has a 405 nm laser light source with a FWHM of ~1 nm. All exposures on this tool are made using the pneumatic autofocus system.

Revision as of 13:49, 20 October 2025

UV resist comparison table

Comparison of specifications and feature space of UV photoresists.

Resist AZ 5214E AZ MiR 701 AZ nLOF 2020 AZ 4562 SU-8 TI Spray
Resist tone
  • Positive
  • Negative (image reversal)
Positive Negative Positive Negative
  • Positive
  • Negative (image reversal)
Thickness range 1.5 - 4.2 µm 1.5 - 4 µm 1.5 - 4 µm 5 - 10 µm 1 - 200 µm 0.5 - 5 µm
Coating tool

Automatic coaters:

  • Spin coater: Gamma UV lithography
  • Spin coater: Gamma ebeam & UV

Manual coaters:

  • Spin coater: Labspin 2
  • Spin coater: Labspin 3
  • Spin coater: RCD8
  • Spray coater

Automatic coaters:

  • Spin coater: Gamma UV lithography
  • Spin coater: Gamma ebeam & UV

Manual coaters:

  • Spin coater: Labspin 2
  • Spin coater: Labspin 3
  • Spin coater: RCD8
  • Spray coater

Automatic coaters:

  • Spin coater: Gamma UV lithography

Manual coaters:

  • Spin coater: Labspin 2
  • Spin coater: Labspin 3
  • Spin coater: RCD8
  • Spray coater

Automatic coaters:

  • Spin coater: Gamma ebeam & UV

Manual coaters:

  • Spin coater: Labspin 2
  • Spin coater: Labspin 3
  • Spin coater: RCD8

Manual coaters:

  • Spin coater: RCD8

or

  • Spin coater: Labspin 2
  • Spin coater: Labspin 3

Spray coater

Spectral sensitivity 310 - 420 nm 310 - 445 nm 310 - 380 nm 310 - 445 nm 300 - 375 nm 310 - 440 nm
Exposure tool Mask aligner or Maskless aligner
Developer
  • AZ 351B
  • AZ 726 MIF
  • AZ 351B
  • AZ 726 MIF
AZ 726 MIF mr-DEV 600 (PGMEA) AZ 726 MIF
Rinse DIW DIW DIW DIW IPA DIW
Remover
  • Acetone
  • Remover 1165
  • Acetone
  • Remover 1165
  • Acetone
  • Remover 1165

Remover 1165

Cured SU-8 is practically insoluble

Plasma ashing can remove crosslinked SU-8

  • Acetone
  • Remover 1165
Comments
  • Can be used for both positive and image reversed (negative) processes with resist thickness between 1 and 4 µm.
  • Good adhesion for wet etch.

High selectivity for dry etch

Negative sidewalls for lift-off

For processes with resist thickness between 6 µm and 25 µm

  • High aspect ratio
  • Resist thickness 1 µm to several 100 µm
  • Available in cleanroom: 2005, 2035, and 2075. Considering discontinuation of the SU-8 2000 series we need to move to another product SU8 3000 and SU8 XTF series.
  • New formulation will be available in cleanroom and tested: 3005 instead of 2005, 3035 instead of 2035, XTF75 instead of 2075 and new 3025.

Spray coater specific resist

Process flow examples

Mask aligner:
Process flow AZ 5214E positive‎ MA6
Process flow AZ 5214E image reversal MA6


Maskless aligner:
Process flow AZ 5214E positive‎ MLA
Process flow AZ 5214E image reversal MLA

Mask aligner:
Process flow AZ MiR 701‎ MA6


Maskless aligner:
Process flow AZ MiR 701‎ MLA

Mask aligner:
Process flow AZ nLOF 2020‎ MA6‎


Maskless aligner:
Process flow AZ nLOF 2020‎ MLA‎

Mask aligner:
Process flow AZ 4562 MA6‎


Maskless aligner:
Process flow AZ 4562 MLA

Mask aligner:
Process flow SU-8 MA6‎


Maskless aligner:
Process flow SU-8 MLA‎


NB! Most of the process knowledge on SU-8 is based in research groups

TI spray resist is an image reversal resist, similar to AZ 5214E. The process flow will be similar to the process flows for 5214, except for the coating step. The exposure dose and development will depend on the specific process.


Other process flows:

Chip on carrier: A procedure for UV lithography on a chip using automatic coater and developer.

Exposure dose

Spectral sensitivity of AZ resists represented as optical absorption coefficient.

During exposure of the resist, the photoinitiator, or photo-active component, reacts with the exposure light, and starts the reaction which makes the resist develop in the developer.

In a positive resist, it makes the resist become soluble in the developer. In a negative resist, usually assisted by thermal energy in the post-exposure bake (PEB), it makes the resist insoluble in the developer. The amount of light required to fully develop the resist in the development process, is the exposure dose.

The optimal exposure dose is a function of many parameters, including the type of resist, the resist thickness, and the sensitivity of the resist.

Resist sensitivity
The resist sensitivity is a measure of how efficiently it reacts to the exposure light. Spectral sensitivity is the sensitivity of the resist as a function of wavelength. It is usually given simply as the range from the wavelength below which absorption in the resist material makes lithography impractical to the wavelength at which the photoinitiator is no longer efficiently activated.

Within the sensitivity range, the optical absorption is commonly used as a measure of sensitivity. A high absorption coefficient signifies a high sensitivity, as the light is absorbed by the photoinitiator. Because of spectral sensitivity, the optimal dose of a given resist type and thickness is also a function of the spectral distribution of the exposure light, i.e. the equipment used for the exposure. Using a combination of experience, calculation and assumptions, it may be possible to estimate the dose for an exposure equipment, if the exposure dose is already known on another equipment.

Due to reflection and refraction at the interface between the resist and the substrate, the optimal dose may also be a function of the type of substrate used. Unless otherwise stated, the exposure doses given below are for standard silicon wafers.

Apart from the already mentioned factors, the optimal dose also depends on the developer chemistry and the parameters used in the development process. Finally, the requirements to the lithographic process in terms of resolution, bias (line broadening), etch selectivity, side wall angle, etc. may narrow down, or widen, the process window. The exposure doses given in the sections below should be used as a starting point for individual fabrication process development.

Due to the process of bleaching, where the absorption of the resist changes during exposure, the exposure dose is unfortunately not always constant at different intensities of the exposure light. The exposure time is thus not always a linear function of the exposure intensity.

Calculate exposure time

In the maskless aligners, the dose is set directly as a process parameter in the job. In mask aligners, on the other hand, the parameter that is set is the exposure time, i.e. how long the shutter is open during the exposure.

The exposure dose, D [J/m2], in terms if exposure light intensity I [W/m2] and exposure time t [s], is given by:

D=I⋅t

Since the intensity is specific to the spectral sensitivity of the sensor used to measure the exposure light, and the exposure time is specific to the spectral distribution of the exposure light (cf. spectral sensitivity), this dose is specific to the combination of exposure source and optical sensor.

Given an exposure dose, the exposure time, t, is calculated as:

t=D⋅I−1

It is important to keep in mind that this exposure time is valid only for a specific combination of exposure source and optical sensor, as well as for a specific development process.

Exposure dose for mask aligners

The exposure doses listed below are for generic good exposure results, and can be a compromise between getting good lines, as well as good dots, in both clear field and dark field exposures. The optimal dose for any given specific project, could be different from the listed values.

All doses are for standard silicon wafers, unless otherwise stated. Development is done using 2.38% TMAH (AZ 726 MIF).


Aligner: MA6-1

The Aligner: MA6-1 has an i-line notch filter installed. This results in an exposure light peak around 365 nm with a FWHM of 7 nm.

Date Thickness Dose Development Comments
AZ 5214E
Data from discontinued German version
Long ago 1.5 µm 72 mJ/cm2 Single puddle, 60 s Positive process
Long ago 2.2 µm 80 mJ/cm2
Long ago 4.2 µm 160 mJ/cm2
AZ 4562
Data from discontinued German version
Long ago 10 µm 510 mJ/cm2 Multiple puddle, 4 x 60 s Multiple exposure with 10-15 s pauses is recommended.
AZ MiR 701
Data from discontinued PFOA containing version
Long ago 1 µm 180 mJ/cm2 Single puddle, 60 s PEB: 60 s at 110°C
Long ago 2 µm 200 mJ/cm2 Single puddle, 60 s
Long ago 4 µm 400 mJ/cm2 Single puddle, 60 s PEB: 90 s at 110°C
AZ nLOF 2020 Long ago 2 µm 110 mJ/cm2 Single puddle, 60 s PEB: 60 s at 110°C

Side wall angle ~15°

For smaller angle (~5°), develop 30 seconds instead


Aligner: MA6-2

The Aligner: MA6-2 has an i-line notch filter installed. This results in an exposure light peak around 365 nm with a FWHM of 7 nm.

New resists
As of 2023-03-21 we no longer have any of the old versions of the resists: AZ 5214E, AZ 4562, AZ MiR 701. The following table contains only information about the new resist versions.

Date Thickness Dose Development Comments
AZ MiR 701 2023-09-26
taran
1.5 µm 150 mJ/cm2

(13.5s @ 11mW/cm2)

Single puddle, 60 s PEB: 60 s @ 110°C
AZ nLOF 2020 2023-09-26
taran
2 µm 121 mJ/cm2

(11 s @ 11 mW/cm2)

Single puddle, 60 s PEB: 60 s @ 110°C
60 s development for lift-off
AZ 5214E

2023-01-11
2025-09-30
jehem

1.5 µm

70 mJ/cm2
90 mJ/cm2

Single puddle, 60 s

Resolution: ~1.5 um

AZ 5214E
Image Reversal
2023-01-11
jehem
2.2 µm 22 mJ/cm2 Single puddle, 60 s

Reversal bake: 60 s at 110°C
Flood exposure: 500 mJ/cm2

AZ 4562
2021-12-08
jehem
10 µm 550 mJ/cm2 Multiple puddles, 5 x 60 s

Priming: HMDS
Rehydration after SB: 1 hour (may not be necessary)
Exposure: Multiple exposures with pauses, 5 x (10 s exposure + 10 s pause)
Degassing after exposure: 1 hour (may not be necessary)


Exposure dose for maskless aligners

The exposure doses listed below are for generic good exposure results, and can be a compromise between getting good lines, as well as good dots, in both clear field and dark field exposures. The optimal dose and achievable resolution for any given specific project, could be different from the listed values.

All doses are for standard silicon wafers, unless otherwise stated. Development is done using 2.38% TMAH (AZ 726 MIF).


Aligner: Maskless 01

The Aligner: Maskless 01 has a 365 nm LED light source with a FWHM of 8 nm.

New resists
As of 2023-03-21 we no longer have any of the old versions of the resists: AZ 5214E, AZ 4562, AZ MiR 701. The following table contains only information about the new resist versions.

Date Thickness Exposure mode Dose Defoc Resolution Comments
AZ MiR 701 2023-07-06
2025-10-16
jehem
1.5 µm Fast 275 mJ/cm2
325 mJ/cm2
1
-1
1 µm
1.5 µm
Tested using dehydration reducing measures
PEB: 60s@110°C
Dev: SP60s
AZ nLOF 2020 2023-07-06
jehem
2.0 µm Fast 180 mJ/cm2 0 1.5 µm PEB: 60s@110°C
Dev: SP60s
AZ 5214E 2024-11-29
2025-08-15
taran
1.5 µm Fast 105 mJ/cm2
110 mJ/cm2
3
-1
1.75 µm Dev: SP60s
See QC data for latest values
AZ 5214E
image reversal
2023-04-05
jehem
2.2 µm Fast possibly obsolete data
20 mJ/cm2
possibly obsolete data
-2
2.0 µm Reversal bake: 60s@110°C,
Flood exposure: 500mJ/cm2
Dev: SP60s
AZ 4562 2023-04-05
jehem
10 µm Fast possibly obsolete data
1050 mJ/cm2
possibly obsolete data
-1
≤5 µm

Priming: HMDS
Rehydration after SB: 1 hour (may not be necessary)
Exposure: Single exposure
Degassing after exposure: 1 hour (may not be necessary)
Development: Multiple puddles, 5 x 60 s


Dehydration reducing measures used for testing AZ MiR 701:
The CDA used for the pneumatic autofocus will dehydrate the resist. To reduce this effect, the writehead is parked far away from the write area while setting up the job for at least a few minutes, before starting the exposure.


Aligner: Maskless 02

The Aligner: Maskless 02 has a 375 nm laser light source with a FWHM of ~1 nm. All exposures on this tool are made using the optical autofocus system, unless otherwise specified.

Quality control
Please note that the values listed in the table are not routinely tested as part of quality control, except for the resist AZ 5214E.

Date Operator Film thickness Exposure mode Dose Defoc Resolution Comments
AZ MIR 701 2023-08-21 taran 1.5 µm Quality 325 mJ/cm2 1 1 µm Not under regular quality control

Post exposure bake: 60 s @ 110°C
Development: 60 s puddle

Tested using dehydration reducing measures
AZ 5214E 2024-12-09 taran 1.5 µm Quality 100 mJ/cm2 2 1.5 µm See QC data for latest values

Development: 60 s puddle
AZ 5214E
Image reversal
2023-04-17 jehem 2.2 µm Quality 35 mJ/cm2 0 1.5 µm Not under regular quality control

Reversal bake: 60 s @ 110°C
Flood exposure: 500 mJ/cm2
Development: 60 s puddle
AZ nLOF 2020 2023-08-21 taran 2.0 µm Quality 450 mJ/cm2 0 1.5 µm Not under regular quality control

Post exposure bake: 60 s @ 110°C
Development: 60 s puddle
AZ 4562 2023-04-19 jehem 10 µm Quality 1150 mJ/cm2 0 ≤5 µm Not under regular quality control

Priming: HMDS
Rehydration after SB: none
Exposure: Single exposure
Degassing after exposure: none
Development: 5 x 60 s multi puddle

New writehead
As of 2023-03-21 the MLA2 has a new writehead installed, converting it from a write mode 1 tool to a write mode 2 tool. This makes all previous dose/defocus settings obsolete. This table contains only the dose/defocus values for the new writehead.

New resists version in 2023
As of 2023-03-21 we no longer have any of the old versions of the resists: AZ 5214E, AZ 4562, AZ MiR 701. This table contains only information about the new resist versions.

Dehydration reducing measures used for testing AZ MiR 701:
The CDA used for the pneumatic autofocus will dehydrate the resist. To reduce this effect, the writehead is parked far away from the write area while setting up the job for at least a few minutes, before starting the exposure.


Aligner: Maskless 03

The Aligner: Maskless 03 has a 405 nm laser light source with a FWHM of ~1 nm. All exposures on this tool are made using the pneumatic autofocus system.

Quality control
Please note that the values listed in the table are not routinely tested as part of quality control, except for the resist AZ 5214E.

Date Operator Film thickness Exposure mode Dose Defoc Resolution Comments
AZ MIR 701 2025-10-20 jehem 1.5 µm Quality 175 mJ/cm2 -1 1 µm Not under regular quality control

Post exposure bake: 60 s @ 110°C
Development: 60 s puddle

Tested using dehydration reducing measures
AZ 5214E 2025-09-02 taran 1.5 µm Quality 75 mJ/cm2 1 1 µm See QC data for latest values

Development: 60 s puddle
AZ 5214E
Image reversal
2023-06-30 jehem 2.2 µm Quality 50 mJ/cm2 0 1 µm Not under regular quality control

Reversal bake: 60 s @ 110°C
Flood exposure: 500 mJ/cm2
Development: 60 s puddle
AZ nLOF 2020 2023-06-30 jehem 2 µm Quality 9000 mJ/cm2 2 1 µm Not under regular quality control

Post exposure bake: 60 s @ 110°C
Development: 60 s puddle

Due to the high dose required on this tool, it is recommended to process nLOF on tools with a more appropriate exposure light source
AZ 4562 2023-06-30 jehem 10 µm Quality 550 mJ/cm2 3 ≤5 µm Not under regular quality control

Priming: HMDS
Rehydration after SB: none
Exposure: Single exposure
Degassing after exposure: none
Development: 5 x 60 s multi puddle

New resists version in 2023
As of 2023-03-21 we no longer have any of the old versions of the resists: AZ 5214E, AZ 4562, AZ MiR 701. This table contains only information about the new resist versions.

Dehydration reducing measures used for testing AZ MiR 701:
The CDA used for the pneumatic autofocus will dehydrate the resist. To reduce this effect, the writehead is parked far away from the write area while setting up the job for at least a few minutes, before starting the exposure.


Exposure dose when using AZ 351B developer (NaOH)

The exposure doses listed below are for generic good exposure results, and can be a compromise between getting good lines, as well as good dots, in both clear field and dark field exposures. The optimal dose for any given specific project, could be different from the listed values.

All doses are for standard silicon wafers, unless otherwise stated. Development is done using AZ 351B developer (NaOH) diluted 1:5.


Aligner: MA6-1

The Aligner: MA6-1 has an i-line notch filter installed. This results in an exposure light peak around 365 nm with a FWHM of 7 nm.

Date Thickness Dose Development] Comments
AZ 5214E
Data from discontinued German version
Long ago 1.5 µm 70mJ/cm2 60 s Positive process
Long ago 2.2 µm 72 mJ/cm2 70 s
Long ago 4.2 µm 160 mJ/cm2 180 s
AZ 5214E
Data from discontinued German version
Long ago 1.5 µm 30 mJ/cm2 60 s Image reversal process.

Reversal bake: 100s at 110°C.
Flood exposure after reversal bake: 210 mJ/cm2

Long ago 2.2 µm 35 mJ/cm2 70 s
AZ 4562
Data from discontinued German version