* [[Specific_Process_Knowledge/Lithography/nLOF#Development|Solvent development possible]]
|
AZ 726 MIF (2.38% TMAH)
|
mr-DEV 600 (PGMEA)
|
AZ 726 MIF (2.38% TMAH)
|-
|-
|-style="background:WhiteSmoke; color:black"
! scope=row| Development rinse agent
!Exposure tool
| DIW || DIW || DIW || DIW || IPA || DIW
|align="center" colspan="5"|Mask aligner or Maskless aligner
|-
|-
! scope=row| Remover
|
* Acetone
* Remover 1165 (NMP)
|
* Acetone
* Remover 1165 (NMP)
|
* Acetone
* Remover 1165 (NMP)
|
Remover 1165 (NMP)
|
* Cross-linked SU-8 is practically insoluble
* Oxygen plasma ashing can remove cross-linked SU-8
|
* Acetone
* Remover 1165 (NMP)
|-
|-
|-style="background:silver; color:black"
! scope=row| Comments
!Developer
| Good adhesion for wet etch
| High selectivity for dry etch
| Negative sidewalls for lift-off
| For processes with resist thickness between 6 µm and 25 µm
|
|
*AZ 351B
* High aspect ratio
*AZ 726 MIF
* Resist thickness 1 µm to hundreds of µm
|
* Available in cleanroom: 2005, 2035, and 2075. Considering discontinuation of the SU-8 2000 series we need to move to another product SU8 3000 and SU8 XTF series.
*AZ 351B
* New formulation will be available in cleanroom and tested: 3005 instead of 2005, 3035 instead of 2035, XTF75 instead of 2075 and new 3025.
*AZ 726 MIF
| TI spray resist is an image reversal resist, similar to AZ 5214E. The process flow will be similar to the process flows for 5214, except for the coating step. The exposure dose and development will depend on the specific process.
|AZ 726 MIF
|}
|AZ 726 MIF
|mr-DEV 600 (PGMEA)
|AZ 726 MIF
|-
|-
<br clear="all" />
|-style="background:WhiteSmoke; color:black"
!Rinse
|DIW
|DIW
|DIW
|DIW
|IPA
|DIW
|-
|-
==Process flow examples==
|-style="background:silver; color:black"
Comparison of specifications and feature space of the standard UV photoresists available at DTU Nanolab. These are just examples and may contain obsolete information regarding exposure dose, etc.
!Remover
|
*Acetone
*Remover 1165
|
*Acetone
*Remover 1165
|
*Acetone
*Remover 1165
|
Remover 1165
|
Cured SU-8 is practically insoluble
Plasma ashing can remove crosslinked SU-8
{| class="wikitable"
|
*Acetone
*Remover 1165
|-
|-
! scope=row| Resist
! style="width: 15%;"| AZ 5214E
! style="width: 15%;"| AZ MIR 701
! style="width: 15%;"| AZ nLOF 2020
! style="width: 15%;"| AZ 4562
! style="width: 15%;"| SU-8
! style="width: 15%;"| Ti Spray
|-
|-
|-style="background:WhiteSmoke; color:black"
! scope=row| Maskless aligner
!Comments
|
|
*Can be used for both positive and image reversed (negative) processes with resist thickness between 1 and 4 µm.
* [[media:process_flow_AZ_5214E_positive_MLA_-_2023-02.docx |Process flow AZ 5214E positive MLA]]
*Good adhesion for wet etch.
* [[media:process_flow_AZ_5214E_IR_MLA_-_2023-02.docx |Process flow AZ 5214E image reversal MLA]]
|
|
High selectivity for dry etch
[[media:process_flow_AZ_MiR_701_MLA_-_2023-02.docx|Process flow AZ MiR 701 MLA]]
|
|
Negative sidewalls for lift-off
[[media:process_flow_AZ_nLOF_2020_MLA_-_2023-02.docx|Process flow AZ nLOF 2020 MLA]]
|
|
For processes with resist thickness between 6 µm and 25 µm
[[media:process_flow_AZ_4562_MLA_-_2023-02.docx|Process flow AZ 4562 MLA]]
NB! Most of the process knowledge on SU-8 is based in research groups
|
|
TI spray resist is an image reversal resist, similar to AZ 5214E. The process flow will be similar to the process flows for 5214, except for the coating step. The exposure dose and development will depend on the specific process.
|}
|-
|}
<br>
'''Other process flows:'''
'''Other process flows:'''
[[Media:process_flow_chip_on_carrier_-_2023-02.docx|Chip on carrier]]: A procedure for UV lithography on a chip using automatic coater and developer.
[[Media:process_flow_chip_on_carrier_-_2023-02.docx|Chip on carrier]]: A procedure for UV lithography on a chip using automatic coater and developer.
<br clear="all" />
<br clear="all" />
==Exposure dose==
==Exposure dose==
[[Image:AZ photoresists spectral sensitivity - remake v1.png|400x400px|thumb|Spectral sensitivity of AZ resists represented as optical absorption coefficient.]]
[[Image:resistSensitivity_UV.png|400px|thumb|Spectral sensitivity of AZ resists represented as optical absorption coefficient.]]
During exposure of the resist, the photoinitiator, or photo-active component, reacts with the exposure light, and starts the reaction which makes the resist develop in the developer.
During exposure of the resist, the photoinitiator, or photo-active component, reacts with the exposure light, and starts the reaction which makes the resist develop in the developer.
Line 264:
Line 240:
==Exposure dose for mask aligners==
==Exposure dose for mask aligners==
The exposure doses listed below are for ''generic'' good exposure results, and can be a compromise between getting good lines, as well as good dots, in both clear field and dark field exposures. The optimal dose for any given specific project, could be different from the listed values.
[[Specific Process Knowledge/Lithography/Resist/UVresist/exposureDoseMaskAligners|Information about the exposure dose for mask aligners can be found here.]]
All doses are for standard silicon wafers, unless otherwise stated. Development is done using 2.38% TMAH.
===KS Aligner===
The KS Aligner has an i-line notch filter installed. This results in an exposure light peak around 365 nm with a FWHM of 7 nm.
!rowspan="2"|AZ 5214E<br><span style="color:red">Old German version</span>
|Long ago
|1.5 µm
|72 mJ/cm<sup>2</sup>
|Single puddle, 60 s
|rowspan="2"|Positive process
|-style="background:WhiteSmoke; color:black"
|Long ago
|2.2 µm
|90 mJ/cm<sup>2</sup>
|Single puddle, 60 s
|-
|-
|-style="background:LightGrey; color:black"
!rowspan="2"|AZ 5214E Image Reversal<br><span style="color:red">Old German version</span>
|Long ago
|1.5 µm
|22 mJ/cm<sup>2</sup>
|Single puddle, 60 s
|rowspan="2"|Image reversal process.<br>Reversal bake: 120 s at 110°C.<br>Flood exposure: 200 mJ/cm<sup>2</sup>
|-style="background:LightGrey; color:black"
|Long ago
|2.2 µm
|25 mJ/cm<sup>2</sup>
|Single puddle, 60 s
|-
|-
|-style="background:WhiteSmoke; color:black"
!rowspan="3"|AZ MiR 701<br><span style="color:red">Old PFOA containing version</span>
|Long ago
|1.5 µm
|169 mJ/cm<sup>2</sup>
|Single puddle, 60 s
|rowspan="2"|PEB: 60 s at 110°C
|-style="background:WhiteSmoke; color:black"
|Long ago
|2 µm
|200 mJ/cm<sup>2</sup>
|Single puddle, 60 s
|-style="background:WhiteSmoke; color:black"
|Long ago
|4 µm
|280 mJ/cm<sup>2</sup>
|Single puddle, 60 s
|rowspan="1"|PEB: 60 s at 110°C<br>Process adopted from process logs
|-
|-
|-style="background:LightGrey; color:black"
!AZ nLOF 2020
|Long ago
|1.5 µm
|104 mJ/cm<sup>2</sup>
|Single puddle, 30 s
|PEB: 60 s at 110°C<br>Use 60 s development for lift-off
|-
|-
|-style="background:WhiteSmoke; color:black"
!AZ 5214E<br><span style="color:green">New Japanese version</span>
|2023-01-11<br>jehem
|1.5 µm
|70 mJ/cm<sup>2</sup>
|Single puddle, 60 s
|
|-
|-
|-style="background:LightGrey; color:black"
!AZ 5214E Image Reversal<br><span style="color:green">New Japanese version</span>
|2023-01-11<br>jehem
|2.2 µm
|22 mJ/cm<sup>2</sup>
|Single puddle, 60 s
|Image reversal process.<br>Reversal bake: 60 s at 110°C.<br>Flood exposure: 500 mJ/cm<sup>2</sup>
|-
|-
|-style="background:WhiteSmoke; color:black"
!AZ 4562<br><span style="color:green">New Japanese version</span>
|2021-12-08<br>jehem
|10 µm
|550 mJ/cm<sup>2</sup>
|Multiple puddles, 5 x 60 s
|Priming: HMDS<BR>Rehydration after SB: 1 hour (may not be necessary)<br>Exposure: Multiple exposures with pauses, 5 x (10 s exposure + 10 s pause)<br>Degassing after exposure: 1 hour (may not be necessary)
|-
|-
|-style="background:LightGrey; color:black"
!AZ MiR 701<br><span style="color:green">New PFOA free version</span>
|2021-06-23<br>elkh
|1.5 µm
|150 mJ/cm<sup>2</sup>
|Single puddle, 60 s
|PEB: 60 s at 110°C
|-
|}
<br clear="all" />
==Exposure dose for maskless aligners==
==Exposure dose for maskless aligners==
The exposure doses listed below are for ''generic'' good exposure results, and can be a compromise between getting good lines, as well as good dots, in both clear field and dark field exposures. The optimal dose for any given specific project, could be different from the listed values.
[[Specific Process Knowledge/Lithography/Resist/UVresist/exposureDoseMasklessAligners|Information about the exposure dose for maskless aligners can be found here.]]
All doses are for standard silicon wafers, unless otherwise stated. Development is done using 2.38% TMAH.
===Aligner: Maskless 01===
The Aligner: Maskless 01 has a 365 nm LED light source with a FWHM of 8 nm.
'''New resists'''<br>
As of 2023-03-21 we no longer have any of the old versions of the resists: AZ 5214E, AZ 4562, AZ MiR 701. The following table contains only information about the new resist versions.
Rehydration after SB: 1 hour (may not be necessary)<br>
Exposure: Single exposure<br>
Degassing after exposure: 1 hour (may not be necessary)<br>
Development: Multiple puddles, 5 x 60 s
|-
|}
<br>
'''Dehydration reducing measures used for testing AZ MiR 701:'''<br>
The CDA used for the pneumatic autofocus will dehydrate the resist. To reduce this effect, the writehead is parked far away from the write area while setting up the job for at least a few minutes, before starting the exposure.
<br clear="all" />
===Aligner: Maskless 02===
<!-- The Aligner: Maskless 02 has a 375 nm laser light source, and a 405 nm laser light source, each with a FWHM of ~1 nm. -->
The Aligner: Maskless 02 has a 375 nm laser light source with a FWHM of ~1 nm.
'''New resists'''<br>
As of 2023-03-21 we no longer have any of the old versions of the resists: AZ 5214E, AZ 4562, AZ MiR 701. The following table contains only information about the new resist versions.
'''New writehead'''<br>
As of 2023-03-21 the MLA2 has a new writehead installed, converting it from a write mode 1 tool to a write mode 2 tool. This makes all previous dose/defocus settings obsolete. The following table contains only the dose/defocus values for the new writehead.
|rowspan="2"| 1 µm<br>Tested using dehydration reducing measures
|rowspan="2"|
PEB: 60s @ 110°C<br>
Dev: SP60s
|-style="background:WhiteSmoke; color:black"
| Pneumatic
| 2
|-
|-
|-style="background:silver; color:black"
!rowspan="2"| AZ nLOF 2020
|rowspan="2"| 2023-03-21<br>jehem
|rowspan="2"| 2.0 µm
|rowspan="2"| 375
| Optical
|rowspan="2"| Quality
|rowspan="2"| 700 mJ/cm<sup>2</sup>
| 6
|rowspan="2"| 1.5 µm
|rowspan="2"|
PEB: 60s @ 110°C<br>
Dev: SP60s
|-style="background:silver; color:black"
| Pneumatic
| 2
|-
|-
|-style="background:WhiteSmoke; color:black"
!rowspan="2"| AZ 5214E
|rowspan="2"| 2023-03-21<br>jehem
|rowspan="2"| 1.5 µm
|rowspan="2"| 375
| Optical
|rowspan="2"| Quality
|rowspan="2"| 120 mJ/cm<sup>2</sup>
| 6
|rowspan="2"| 1 µm
|rowspan="2"| Dev: SP60s
|-style="background:WhiteSmoke; color:black"
| Pneumatic
| 2
|-
|-
|-style="background:silver; color:black"
!rowspan="2"| AZ 5214E<br>image reversal
|rowspan="2"| 2023-03-21<br>jehem
|rowspan="2"| 2.2 µm
|rowspan="2"| 375
| Optical
|rowspan="2"| Quality
|rowspan="2"| 45 mJ/cm<sup>2</sup>
| 6
|rowspan="2"| 1.5 µm
|rowspan="2"|
Reversal bake: 60s @ 110°C<br>
Flood exposure: 500 mJ/cm<sup>2</sup><br>
Dev: SP60s
|-style="background:silver; color:black"
| Pneumatic
| 2
|-
|-
|-style="background:whitesmoke; color:black"
!rowspan="2"| AZ 4562
|rowspan="2"| Not tested yet
|rowspan="2"| 10 µm
|rowspan="2"| 375
| Optical
|rowspan="2"| Quality
|rowspan="2"|
|
|rowspan="2"|
|rowspan="2"|
Priming: HMDS<br>
Rehydration after softbake: 1 hour (may not be necessary)<br>
Exposure: Single exposure<br>
Degassing after exposure: 1 hour (may not be necessary)<br>
Development: Multiple puddles, 5 x 60 s
|-style="background:whitesmoke; color:black"
| Pneumatic
|
|-
|}
<br>
'''Dehydration reducing measures used for testing AZ MiR 701:'''<br>
The CDA used for the pneumatic autofocus will dehydrate the resist. To reduce this effect, the writehead is parked far away from the write area while setting up the job for at least a few minutes, before starting the exposure.
<br clear="all" />
===Aligner: Maskless 03===
The Aligner: Maskless 03 has a 405 nm laser light source with a FWHM of ~1 nm.
'''New resists'''<br>
As of 2023-03-21 we no longer have any of the old versions of the resists: AZ 5214E, AZ 4562, AZ MiR 701. The following table contains only information about the new resist versions.
| 1 µm<br>Tested using dehydration reducing measures
| PEB: 60s@110°C<br>Dev: SP60s
|-
|-
|-style="background:silver; color:black"
!AZ nLOF 2020
| 2023-01-13<br>jehem
| 2.0 µm
| 405
| Pneumatic
| Quality
| 9000 mJ/cm<sup>2</sup>
| 0
| 1 µm
|
PEB: 60s @ 100°C<br>
Dev: SP60s<br>
<span style="color:red">'''Due to the high dose required on this tool, it is recommended to process nLOF on tools with a more appropriate exposure light source'''</span>
|-
|-
|-style="background:WhiteSmoke; color:black"
!AZ 5214E
| 2023-01-06<br>jehem
| 1.5 µm
| 405
| Pneumatic
| Quality
| 70 mJ/cm<sup>2</sup>
| -2
| 1 µm
| Dev: SP60s
|-
|-
|-style="background:silver; color:black"
!AZ 5214E<br>Image reversal
| 2023-01-06<br>jehem
| 2.2 µm
| 405
| Pneumatic
| Quality
| 50 mJ/cm<sup>2</sup>
| -2
| 1 µm
|
Reversal bake: 60s@110°C<br>
Flood exposure: 500mJ/cm<sup>2</sup><br>
Dev: SP60s
|-
|-
|-style="background:whitesmoke; color:black"
!AZ 4562
| 2021-12-08<br>jehem
| 10 µm
| 405
| Pneumatic
| Quality
| 550 mJ/cm<sup>2</sup>
| 1
| ≤5 µm
|
Priming: HMDS<BR>
Rehydration after SB: 1 hour (may not be necessary)<br>
Exposure: Single exposure<br>
Degassing after exposure: 1 hour (may not be necessary)<br>
Development: Multiple puddles, 5 x 60 s
|-
|}
<br>
'''Dehydration reducing measures used for testing AZ MiR 701:'''<br>
The CDA used for the pneumatic autofocus will dehydrate the resist. To reduce this effect, the writehead is parked far away from the write area while setting up the job for at least a few minutes, before starting the exposure.
<br clear="all" />
==Exposure dose when using AZ 351B developer (NaOH)==
==Exposure dose when using AZ 351B developer (NaOH)==
The exposure doses listed below are for ''generic'' good exposure results, and can be a compromise between getting good lines, as well as good dots, in both clear field and dark field exposures. The optimal dose for any given specific project, could be different from the listed values.
[[Specific Process Knowledge/Lithography/Resist/UVresist/exposureDoseNaOH|Information about the exposure dose when using AZ 351B developer can be found here.]]
All doses are for standard silicon wafers, unless otherwise stated. Development is done using AZ 351B developer (NaOH).
===KS Aligner (351B)===
The KS Aligner has an i-line notch filter installed. This results in an exposure light peak around 365 nm with a FWHM of 7 nm.
For processes with resist thickness between 6 µm and 25 µm
High aspect ratio
Resist thickness 1 µm to hundreds of µm
Available in cleanroom: 2005, 2035, and 2075. Considering discontinuation of the SU-8 2000 series we need to move to another product SU8 3000 and SU8 XTF series.
New formulation will be available in cleanroom and tested: 3005 instead of 2005, 3035 instead of 2035, XTF75 instead of 2075 and new 3025.
TI spray resist is an image reversal resist, similar to AZ 5214E. The process flow will be similar to the process flows for 5214, except for the coating step. The exposure dose and development will depend on the specific process.
Process flow examples
Comparison of specifications and feature space of the standard UV photoresists available at DTU Nanolab. These are just examples and may contain obsolete information regarding exposure dose, etc.
NB! Most of the process knowledge about SU-8 is based in research groups
Other process flows:Chip on carrier: A procedure for UV lithography on a chip using automatic coater and developer.
Exposure dose
Spectral sensitivity of AZ resists represented as optical absorption coefficient.
During exposure of the resist, the photoinitiator, or photo-active component, reacts with the exposure light, and starts the reaction which makes the resist develop in the developer.
In a positive resist, it makes the resist become soluble in the developer. In a negative resist, usually assisted by thermal energy in the post-exposure bake (PEB), it makes the resist insoluble in the developer. The amount of light required to fully develop the resist in the development process, is the exposure dose.
The optimal exposure dose is a function of many parameters, including the type of resist, the resist thickness, and the sensitivity of the resist.
Resist sensitivity
The resist sensitivity is a measure of how efficiently it reacts to the exposure light. Spectral sensitivity is the sensitivity of the resist as a function of wavelength. It is usually given simply as the range from the wavelength below which absorption in the resist material makes lithography impractical to the wavelength at which the photoinitiator is no longer efficiently activated.
Within the sensitivity range, the optical absorption is commonly used as a measure of sensitivity. A high absorption coefficient signifies a high sensitivity, as the light is absorbed by the photoinitiator. Because of spectral sensitivity, the optimal dose of a given resist type and thickness is also a function of the spectral distribution of the exposure light, i.e. the equipment used for the exposure. Using a combination of experience, calculation and assumptions, it may be possible to estimate the dose for an exposure equipment, if the exposure dose is already known on another equipment.
Due to reflection and refraction at the interface between the resist and the substrate, the optimal dose may also be a function of the type of substrate used. Unless otherwise stated, the exposure doses given below are for standard silicon wafers.
Apart from the already mentioned factors, the optimal dose also depends on the developer chemistry and the parameters used in the development process. Finally, the requirements to the lithographic process in terms of resolution, bias (line broadening), etch selectivity, side wall angle, etc. may narrow down, or widen, the process window. The exposure doses given in the sections below should be used as a starting point for individual fabrication process development.
Due to the process of bleaching, where the absorption of the resist changes during exposure, the exposure dose is unfortunately not always constant at different intensities of the exposure light. The exposure time is thus not always a linear function of the exposure intensity.
Calculate exposure time
In the maskless aligners, the dose is set directly as a process parameter in the job. In mask aligners, on the other hand, the parameter that is set is the exposure time, i.e. how long the shutter is open during the exposure.
The exposure dose, D [J/m2], in terms if exposure light intensity I [W/m2] and exposure time t [s], is given by:
Since the intensity is specific to the spectral sensitivity of the sensor used to measure the exposure light, and the exposure time is specific to the spectral distribution of the exposure light (cf. spectral sensitivity), this dose is specific to the combination of exposure source and optical sensor.
Given an exposure dose, the exposure time, t, is calculated as:
It is important to keep in mind that this exposure time is valid only for a specific combination of exposure source and optical sensor, as well as for a specific development process.