'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Resist/UVresist click here]'''
'''This section is under construction [[Image:section under construction.jpg|70px]]'''
==UV resist comparison table==
==UV resist comparison table==
Comparison of specifications and feature space of UV photoresists.
Comparison of specifications and feature space of the standard UV photoresists available at DTU Nanolab.
 
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;"
|-


{| class="wikitable"
|-
|-
|-style="background:silver; color:black"
! scope=row| Resist
!Resist
! style="width: 15%;"| [[Specific_Process_Knowledge/Lithography/5214E|AZ 5214E]]
|AZ 5214E
! style="width: 15%;"| [[Specific_Process_Knowledge/Lithography/MiR|AZ MiR 701]]
|AZ MiR 701
! style="width: 15%;"| [[Specific_Process_Knowledge/Lithography/nLOF|AZ nLOF 2020]]
|AZ nLOF 202
! style="width: 15%;"| [[Specific_Process_Knowledge/Lithography/4562|AZ 4562]]
|AZ 4562
! style="width: 15%;"| [[Specific_Process_Knowledge/Lithography/SU-8|SU-8]]
|SU-8 20xx
! style="width: 15%;"| [[Specific_Process_Knowledge/Lithography/TIspray|TI Spray]]
|-
|-
 
! scope=row| Resist tone
|-
|
|-style="background:WhiteSmoke; color:black"
*Positive
!Resist tone
*Negative (image reversal)
|
| Positive
| Negative
| Positive
| Negative
|  
*Positive
*Positive
*Negative (image reversal)
*Negative (image reversal)
|Positive
|Negative
|Positive
|Negative
|-
|-
! scope=row| Thickness range
| 1.5 - 4.2 µm || 1.5 - 4 µm || 1.5 - 4 µm  || 5 - 10 µm || 1 - 200 µm || 0.5 - 5 µm
|-
! scope=row| Coating tool
|
Automatic spin coaters:
*Spin coater: Gamma UV lithography
*Spin coater: Gamma E-beam & UV


|-style="background:silver; color:black"
Manual spin coaters:
!Thickness range
* Spin coater: Labspin 02
|1.5 - 4.2 µm
* Spin coater: Labspin 03
|1.5 - 4 µm
* Spin coater: RCD8
|1.5 - 4 µm
|5 - 10 µm
|1 - 200 µm
|-


|-
Spray coater
|-style="background:WhiteSmoke; color:black"
|  
!Coating tool
Automatic spin coaters:
|
Automatic coaters:<br>
*Spin coater: Gamma UV lithography
*Spin coater: Gamma UV lithography
*Spin coater: Gamma ebeam & UV
*Spin coater: Gamma E-beam & UV  
 
Manual spin coaters:
* Spin coater: Labspin 02
* Spin coater: Labspin 03
* Spin coater: RCD8


Manual coaters:<br>
Spray coater
*Spin coater: Labspin 2
|  
*Spin coater: Labspin 3
Automatic spin coaters:
*Spin coater: RCD8
*Spray coater
|
Automatic coaters:<br>
*Spin coater: Gamma UV lithography
*Spin coater: Gamma UV lithography
*Spin coater: Gamma ebeam & UV


Manual coaters:<br>
Manual spin coaters:
*Spin coater: Labspin 2
* Spin coater: Labspin 02
*Spin coater: Labspin 3
* Spin coater: Labspin 03
*Spin coater: RCD8
* Spin coater: RCD8
*Spray coater
 
Spray coater
|
Automatic spin coaters:
*Spin coater: Gamma E-beam & UV
 
Manual spin coaters:
* Spin coater: Labspin 02
* Spin coater: Labspin 03
* Spin coater: RCD8
|
Manual spin coaters:
* Spin coater: Labspin 02
* Spin coater: Labspin 03
* Spin coater: RCD8
|
Spray coater
|-
! scope=row| Spectral sensitivity
| 310 - 420 nm || 310 - 445 nm || 310 - 380 nm || 310 - 445 nm || 300 - 375 nm || 310 - 440 nm
|-
! scope=row| Exposure tool
|
* Maskless aligners
* Mask aligners
|
* Maskless aligners
* Mask aligners
|
* Maskless aligners
* Mask aligners
|
* Maskless aligners
* Mask aligners
|
* Maskless aligners
* Mask aligners
|
* Maskless aligners
* Mask aligners
|-
! scope=row| Developer
|
* AZ 726 MIF (2.38% TMAH)
* AZ 351 B (NaOH)
|
* AZ 726 MIF (2.38% TMAH)
* AZ 351 B (NaOH)
|
* AZ 726 MIF (2.38% TMAH)
* [[Specific_Process_Knowledge/Lithography/nLOF#Development|Solvent development possible]]
|
AZ 726 MIF (2.38% TMAH)
|
mr-DEV 600 (PGMEA)
|
AZ 726 MIF (2.38% TMAH)
|-
! scope=row| Development rinse agent
| DIW || DIW || DIW || DIW || IPA || DIW
|-
! scope=row| Remover
|
* Acetone
* Remover 1165 (NMP)
|
* Acetone
* Remover 1165 (NMP)
|
* Acetone
* Remover 1165 (NMP)
|
Remover 1165 (NMP)
|
* Cross-linked SU-8 is practically insoluble
* Oxygen plasma ashing can remove cross-linked SU-8
|
* Acetone
* Remover 1165 (NMP)
|-
! scope=row| Comments
| Good adhesion for wet etch
| High selectivity for dry etch
| Negative sidewalls for lift-off
| For processes with resist thickness between 6 µm and 25 µm
|
|
Automatic coaters:<br>
* High aspect ratio
*Spin coater: Gamma UV lithography
* Resist thickness 1 µm to hundreds of µm
* Available in cleanroom: 2005, 2035, and 2075. Considering discontinuation of the SU-8 2000 series we need to move to another product SU8 3000 and SU8 XTF series.
* New formulation will be available in cleanroom and tested: 3005 instead of 2005, 3035 instead of 2035, XTF75 instead of 2075 and new 3025.
| TI spray resist is an image reversal resist, similar to AZ 5214E. The process flow will be similar to the process flows for 5214, except for the coating step. The exposure dose and development will depend on the specific process.
|}
 
<br clear="all" />
 
==Process flow examples==
Comparison of specifications and feature space of the standard UV photoresists available at DTU Nanolab. These are just examples and may contain obsolete information regarding exposure dose, etc.


Manual coaters:<br>
{| class="wikitable"
*Spin coater: Labspin 2
|-
*Spin coater: Labspin 3
! scope=row| Resist
*Spin coater: RCD8
! style="width: 15%;"| AZ 5214E
*Spray coater
! style="width: 15%;"| AZ MIR 701
! style="width: 15%;"| AZ nLOF 2020
! style="width: 15%;"| AZ 4562
! style="width: 15%;"| SU-8
! style="width: 15%;"| Ti Spray
|-
! scope=row| Maskless aligner
|
|
Automatic coaters:<br>
* [[media:‎process_flow_AZ_5214E_positive_MLA_-_2023-02.docx‎ |Process flow AZ 5214E positive‎ MLA]]
*Spin coater: Gamma ebeam & UV
* [[media:process_flow_AZ_5214E_IR_MLA_-_2023-02.docx‎ |Process flow AZ 5214E image reversal MLA]]
|
[[media:process_flow_AZ_MiR_701_MLA_-_2023-02.docx‎|Process flow AZ MiR 701‎ MLA]]
|
[[media:process_flow_AZ_nLOF_2020_MLA_-_2023-02.docx‎|Process flow AZ nLOF 2020‎ MLA‎]]
|
[[media:process_flow_AZ_4562_MLA_-_2023-02.docx‎|Process flow AZ 4562 MLA]]
|
[[media:process_flow_SU-8_MLA_-_2023-02.docx‎|Process flow SU-8 MLA‎]]


Manual coaters:<br>
NB! Most of the process knowledge about SU-8 is based in research groups
*Spin coater: Labspin 2
*Spin coater: Labspin 3
*Spin coater: RCD8
|
|
Manual coaters:<br>
*Spin coater: RCD8
|-
|-
! scope=row| Mask aligner
|
* [[media:‎process_flow_AZ_5214E_positive_MA6_-_2023-02.docx‎ |Process flow AZ 5214E positive‎ MA6]]
* [[media:process_flow_AZ_5214E_IR_MA6_-_2023-02.docx‎ |Process flow AZ 5214E image reversal MA6]]
|
[[media:process_flow_AZ_MiR_701_MA6_-_2023-02.docx‎|Process flow AZ MiR 701‎ MA6]]
|
[[media:process_flow_AZ_nLOF_2020_MA6_-_2023-02.docx‎|Process flow AZ nLOF 2020‎ MA6‎]]
|
[[media:process_flow_AZ_4562_MA6_-_2023-02.docx‎|Process flow AZ 4562 MA6‎]]
|
[[media:process_flow_SU-8_MA6_-_2023-02.docx‎|Process flow SU-8 MA6‎]]


NB! Most of the process knowledge about SU-8 is based in research groups
|
|}
|}
'''Other process flows:'''
[[Media:process_flow_chip_on_carrier_-_2023-02.docx|Chip on carrier]]: A procedure for UV lithography on a chip using automatic coater and developer.
<br clear="all" />
<br clear="all" />


==Exposure dose==
==Exposure dose==
[[Image:AZ photoresists spectral sensitivity - remake v1.png|400x400px|thumb|Spectral sensitivity of AZ resists represented as optical absorption.]]
[[Image:resistSensitivity_UV.png|400px|thumb|Spectral sensitivity of AZ resists represented as optical absorption coefficient.]]


During exposure of the resist, the photoinitiator, or photo-active component, reacts with the exposure light, and starts the reaction that makes the resist develop in the developer.
During exposure of the resist, the photoinitiator, or photo-active component, reacts with the exposure light, and starts the reaction which makes the resist develop in the developer.


In a positive resist, it makes the resist become soluble in the developer. In a negative resist, usually assisted by thermal energy in the post-exposure bake, it makes the resist ''in''soluble in the developer. The amount of light required to fully develop the resist in the development process, is the exposure dose.
In a positive resist, it makes the resist become soluble in the developer. In a negative resist, usually assisted by thermal energy in the post-exposure bake (PEB), it makes the resist ''in''soluble in the developer. The amount of light required to fully develop the resist in the development process, is the exposure dose.


The optimal exposure dose is a function of many parameters, including the type of resist, the resist thickness, and the sensitivity of the resist.
The optimal exposure dose is a function of many parameters, including the type of resist, the resist thickness, and the sensitivity of the resist.
Line 111: Line 227:
In the maskless aligners, the dose is set directly as a process parameter in the job. In mask aligners, on the other hand, the parameter that is set is the exposure time, i.e. how long the shutter is open during the exposure.
In the maskless aligners, the dose is set directly as a process parameter in the job. In mask aligners, on the other hand, the parameter that is set is the exposure time, i.e. how long the shutter is open during the exposure.


The exposure dose, ''D'' [J/m<sup>2</sup>], is given by:
The exposure dose, ''D'' [J/m<sup>2</sup>], in terms if exposure light intensity ''I'' [W/m<sup>2</sup>] and exposure time ''t'' [s], is given by:


''D'' = ''I'' x ''t'' ,
<math>D=I \sdot t</math>


where ''I'' [W/m<sup>2</sup>] is the intensity of the exposure light, and ''t'' [s] is the exposure time. As the intensity is specific to the spectral sensitivity of the sensor used to measure the exposure light, and the exposure time is specific to the spectral distribution of the exposure light (cf. spectral sensitivity), this dose is specific to the combination of exposure source and optical sensor.
Since the intensity is specific to the spectral sensitivity of the sensor used to measure the exposure light, and the exposure time is specific to the spectral distribution of the exposure light (cf. spectral sensitivity), this dose is specific to the combination of exposure source and optical sensor.


Given an exposure dose, the exposure time, ''t'', is calculated as:
Given an exposure dose, the exposure time, ''t'', is calculated as:


''t'' = ''D'' / ''I''
<math>t = D \sdot I^{-1}</math>


It is important to keep in mind that this exposure time is valid only for a specific combination of exposure source and optical sensor, as well as for a specific development process.
It is important to keep in mind that this exposure time is valid ''only'' for a specific combination of exposure source and optical sensor, as well as for a specific development process.


==Exposure dose for mask aligners==
==Exposure dose for mask aligners==
The exposure doses listed below are for ''generic'' good exposure results, and can be a compromise between getting good lines, as well as good dots, in both clear field and dark field exposures. The optimal dose for any given specific project, could be different from the listed values.
The exposure doses listed below are for ''generic'' good exposure results, and can be a compromise between getting good lines, as well as good dots, in both clear field and dark field exposures. The optimal dose for any given specific project, could be different from the listed values.


All doses are for standard silicon wafers, unless otherwise stated. Development is done using 2.38% TMAH.
All doses are for standard silicon wafers, unless otherwise stated. Development is done using 2.38% TMAH (AZ 726 MIF).


===KS Aligner===
The KS Aligner has an i-line notch filter installed. This results in an exposure light peak around 365 nm with a FWHM of 7 nm.


{|border="1" cellspacing="1" cellpadding="7" style="text-align:left;"
===Aligner: MA6-1===
|-
The Aligner: MA6-1 has an i-line notch filter installed. This produces an exposure light peak around 365 nm with a FWHM of 7 nm.


|-
'''Quality control'''<br>
|-style="background:silver; color:black"
Please note that the values listed in the table are <i>'''not'''</i> routinely tested as part of quality control.
|
!Date
!Thickness
!Dose
!Development
!Comments
|-


{| class="wikitable"
|-
|-
|-style="background:WhiteSmoke; color:black"
! !! Date !! Operator !! Film thickness !! Exposure mode !! Dose !! Resolution !! Comments
!rowspan="3"|AZ 5214E<br><span style="color:red">Old German version</span>
|Long ago
|1.5 µm
|72 mJ/cm<sup>2</sup>
|rowspan="3"|Single puddle, 60 s
|rowspan="3"|Positive process
|-style="background:WhiteSmoke; color:black"
|Long ago
|2.2 µm
|80 mJ/cm<sup>2</sup>
|-style="background:WhiteSmoke; color:black"
|Long ago
|4.2 µm
|160 mJ/cm<sup>2</sup>
|-
|-
 
! scope=row| AZ MIR 701
| Long ago || ? || 1.5 µm || ? || 180 mJ/cm<sup>2</sup> || ? µm || '''Not under regular quality control'''<br><br>Post exposure bake: 60 s @ 110°C<br>Development: 60 s puddle
|-
|-
|-style="background:LightGrey; color:black"
! scope=row| AZ MIR 701
!AZ 4562<br><span style="color:red">Old German version</span>
| Long ago || ? || 2.0 µm || ? || 200 mJ/cm<sup>2</sup> || ? µm || '''Not under regular quality control'''<br><br>Post exposure bake: 60 s @ 110°C<br>Development: 60 s puddle
|Long ago
|10 µm
|510 mJ/cm<sup>2</sup>
|Multiple puddle, 4 x 60 s
|Multiple exposure with 10-15 s pauses is recommended.
|-
|-
 
! scope=row| AZ MIR 701
| Long ago || ? || 4.0 µm || ? || 400 mJ/cm<sup>2</sup> || ? µm || '''Not under regular quality control'''<br><br>Post exposure bake: 60 s @ 110°C<br>Development: 60 s puddle
|-
|-
|-style="background:WhiteSmoke; color:black"
! scope=row| AZ 5214E
!rowspan="3"|AZ MiR 701<br><span style="color:red">Old PFOA containing version</span>
| Long ago || ? || 1.5 µm || ? || 72 mJ/cm<sup>2</sup> || ? µm || '''Not under regular quality control'''<br><br>Development: 60 s puddle
|Long ago
|1 µm
|180 mJ/cm<sup>2</sup>
|Single puddle, 60 s
|rowspan="2"|PEB: 60 s at 110°C
|-style="background:WhiteSmoke; color:black"
|Long ago
|2 µm
|200 mJ/cm<sup>2</sup>
|Single puddle, 60 s
|-style="background:WhiteSmoke; color:black"
|Long ago
|4 µm
|400 mJ/cm<sup>2</sup>
|Single puddle, 60 s
|rowspan="1"|PEB: 90 s at 110°C
|-
|-
 
! scope=row| AZ 5214E
| Long ago || ? || 2.2 µm || ? || 80 mJ/cm<sup>2</sup> || ? µm || '''Not under regular quality control'''<br><br>Development: 60 s puddle
|-
|-
|-style="background:LightGrey; color:black"
! scope=row| AZ 5214E
!AZ nLOF 2020
| Long ago || ? || 4.2 µm || ? || 160 mJ/cm<sup>2</sup> || ? µm || '''Not under regular quality control'''<br><br>Development: 60 s puddle
|Long ago
|2 µm
|110 mJ/cm<sup>2</sup>
|Single puddle, 60 s
|PEB: 60 s at 110°C
Side wall angle ~15°
 
For smaller angle (~5°), develop 30 seconds instead
|}
 
===Aligner: MA6 - 2===
The Aligner: MA6-2 has an i-line notch filter installed. This results in an exposure light peak around 365 nm with a FWHM of 7 nm.
 
{|border="1" cellspacing="1" cellpadding="7" style="text-align:left;"
|-
|-
 
! scope=row| AZ 5214E<br>Image reversal
| Long ago || ? || 2.2 µm || ? || ? mJ/cm<sup>2</sup> || ? µm || '''Not under regular quality control'''<br><br>Reversal bake: 60 s @ 110°C<br>Flood exposure: 500 mJ/cm<sup>2</sup><br>Development: 60 s puddle
|-
|-
|-style="background:silver; color:black"
! scope=row| AZ nLOF 2020
|
| Long ago || ? || 2.0 µm || ? || 121 mJ/cm<sup>2</sup> || ? µm || '''Not under regular quality control'''<br><br>Post exposure bake: 60 s @ 110°C<br>Development: 60 s puddle<br><br>Side wall angle: ~15°<br>For smaller angle (~5°): develop 30 seconds instead
!Date
!Thickness
!Dose
!Development
!Comments
|-
 
|-
|-style="background:WhiteSmoke; color:black"
!rowspan="2"|AZ 5214E<br><span style="color:red">Old German version</span>
|Long ago
|1.5 µm
|72 mJ/cm<sup>2</sup>
|Single puddle, 60 s
|rowspan="2"|Positive process
|-style="background:WhiteSmoke; color:black"
|Long ago
|2.2 µm
|90 mJ/cm<sup>2</sup>
|Single puddle, 60 s
|-
|-
! scope=row| AZ 4562
| Long ago || ? || 10 µm || ? || 510 mJ/cm<sup>2</sup> || ≤5 µm || '''Not under regular quality control'''<br><br>Priming: HMDS<BR>Rehydration after SB: none<br>Exposure: Multiple exposures with 15 s pauses is recommended<br>Degassing after exposure: none<br>Development: 5 x 60 s multi puddle
|}


|-
'''New resists version in 2023'''<br>
|-style="background:LightGrey; color:black"
As of 2023-03-21 we no longer have any of the old versions of the resists: AZ 5214E, AZ 4562, AZ MiR 701. <span style="color:red">This table contains only information about the <i>old</i> resist versions.</span>
!rowspan="2"|AZ 5214E Image Reversal<br><span style="color:red">Old German version</span>
|Long ago
|1.5 µm
|22 mJ/cm<sup>2</sup>
|Single puddle, 60 s
|rowspan="2"|Image reversal process.<br>Reversal bake: 120 s at 110°C.<br>Flood exposure: 200 mJ/cm<sup>2</sup>
|-style="background:LightGrey; color:black"
|Long ago
|2.2 µm
|25 mJ/cm<sup>2</sup>
|Single puddle, 60 s
|-


|-
<br clear="all" />
|-style="background:WhiteSmoke; color:black"
!rowspan="3"|AZ MiR 701<br><span style="color:red">Old PFOA containing version</span>
|Long ago
|1.5 µm
|169 mJ/cm<sup>2</sup>
|Single puddle, 60 s
|rowspan="2"|PEB: 60 s at 110°C
|-style="background:WhiteSmoke; color:black"
|Long ago
|2 µm
|200 mJ/cm<sup>2</sup>
|Single puddle, 60 s
|-style="background:WhiteSmoke; color:black"
|Long ago
|4 µm
|280 mJ/cm<sup>2</sup>
|Single puddle, 60 s
|rowspan="1"|PEB: 60 s at 110°C<br>Process adopted from process logs
|-


|-
===Aligner: MA6-2===
|-style="background:LightGrey; color:black"
The Aligner: MA6-2 has an i-line notch filter installed. This produces an exposure light peak around 365 nm with a FWHM of 7 nm.
!AZ nLOF 2020
|Long ago
|1.5 µm
|104 mJ/cm<sup>2</sup>
|Single puddle, 30 s
|PEB: 60 s at 110°C<br>Use 60 s development for lift-off
|-


|-
'''Quality control'''<br>
|-style="background:WhiteSmoke; color:black"
Please note that the values listed in the table are <i>'''not'''</i> routinely tested as part of quality control.
!AZ 5214E<br><span style="color:green">New Japanese version</span>
|2023-01-11<br>jehem
|1.5 µm
|70 mJ/cm<sup>2</sup>
|Single puddle, 60 s
|
|-


{| class="wikitable"
|-
|-
|-style="background:LightGrey; color:black"
! !! Date !! Operator !! Film thickness !! Exposure mode !! Dose !! Resolution !! Comments
!AZ 5214E Image Reversal<br><span style="color:green">New Japanese version</span>
|2023-01-11<br>jehem
|2.2 µm
|22 mJ/cm<sup>2</sup>
|Single puddle, 60 s
|Image reversal process.<br>Reversal bake: 60 s at 110°C.<br>Flood exposure: 500 mJ/cm<sup>2</sup>
|-
|-
 
! scope=row| AZ MIR 701
| 2023-09-26 || taran || 1.5 µm || Hard contact || 150 mJ/cm<sup>2</sup> || ? µm || '''Not under regular quality control'''<br><br>Post exposure bake: 60 s @ 110°C<br>Development: 60 s puddle
|-
|-
|-style="background:WhiteSmoke; color:black"
! scope=row| AZ 5214E
!AZ 4562<br><span style="color:green">New Japanese version</span>
| 2025-09-30 || jehem || 1.5 µm || Hard contact|| 90 mJ/cm<sup>2</sup> || 1.5 µm || '''Not under regular quality control'''<br><br>Development: 60 s puddle
|2021-12-08<br>jehem
|10 µm
|550 mJ/cm<sup>2</sup>
|Multiple puddles, 5 x 60 s
|Priming: HMDS<BR>Rehydration after SB: 1 hour (may not be necessary)<br>Exposure: Multiple exposures with pauses, 5 x (10 s exposure + 10 s pause)<br>Degassing after exposure: 1 hour (may not be necessary)
|-
|-
 
! scope=row| AZ 5214E<br>Image reversal
| 2023-01-11 || jehem || 2.2 µm || Hard contact|| 22 mJ/cm<sup>2</sup> || 2.0 µm || '''Not under regular quality control'''<br><br>Reversal bake: 60 s @ 110°C<br>Flood exposure: 500 mJ/cm<sup>2</sup><br>Development: 60 s puddle
|-
|-
|-style="background:LightGrey; color:black"
! scope=row| AZ nLOF 2020
!AZ MiR 701<br><span style="color:green">New PFOA free version</span>
| 2023-09-26 || taran || 2.0 µm || Hard contact || 121 mJ/cm<sup>2</sup> || ? µm || '''Not under regular quality control'''<br><br>Post exposure bake: 60 s @ 110°C<br>Development: 60 s puddle
|2021-06-23<br>elkh
|1.5 µm
|150 mJ/cm<sup>2</sup>
|Single puddle, 60 s
|PEB: 60 s at 110°C
|-
|-
! scope=row| AZ 4562
| 2021-12-08 || jehem || 10 µm || Soft contact|| 550 mJ/cm<sup>2</sup> || ≤5 µm || '''Not under regular quality control'''<br><br>Priming: HMDS<BR>Rehydration after SB: none<br>Exposure: Single exposure<br>Degassing after exposure: none<br>Development: 5 x 60 s multi puddle
|}
|}


==Exposure dose for maskless aligners==
'''New resists version in 2023'''<br>
The exposure doses listed below are for ''generic'' good exposure results, and can be a compromise between getting good lines, as well as good dots, in both clear field and dark field exposures. The optimal dose for any given specific project, could be different from the listed values.
As of 2023-03-21 we no longer have any of the old versions of the resists: AZ 5214E, AZ 4562, AZ MiR 701. This table contains only information about the new resist versions.


All doses are for standard silicon wafers, unless otherwise stated. Development is done using 2.38% TMAH.
<br clear="all" />


===Aligner: Maskless 01===
==Exposure dose for maskless aligners==
The Aligner: Maskless 01 has a 365 nm LED light source with a FWHM of 8 nm.
The exposure doses listed below are for ''generic'' good exposure results, and can be a compromise between getting good lines, as well as good dots, in both clear field and dark field exposures. The optimal dose and achievable resolution for any given specific project, could be different from the listed values.


{|border="1" cellspacing="1" cellpadding="7" style="text-align:left;"
All doses are for standard silicon wafers, unless otherwise stated. Development is done using 2.38% TMAH (AZ 726 MIF).
|-
 
|-
|-style="background:silver; color:black"
|
!Date
!Thickness
!Exposure mode
!Dose
!Defoc
!Resolution
!Comments
|-


|-
|-style="background:WhiteSmoke; color:black"
!rowspan="2"| AZ 5214E<br><span style="color:red">Old German version</span>
| 2021-08-19<br>jehem
| 1.5 µm
| Fast
| 80 mJ/cm<sup>2</sup>
| -4
| 2 µm
| Dev: SP60s
|-style="background:WhiteSmoke; color:black"
| 2021-08-19<br>jehem
| 1.5 µm
| Quality
| 80 mJ/cm<sup>2</sup>
| -4
| 1.25 µm
| Dev: SP60s
|-


|-
===Aligner: Maskless 01===
|-style="background:LightGrey; color:black"
The Aligner: Maskless 01 has a 365 nm laser light source with a FWHM of ~1 nm. The test exposures on this tool were made using the pneumatic autofocus system.
!rowspan="2"| AZ 5214E image reversal<br><span style="color:red">Old German version</span>
| 2020-03-01<br>taran
| 2.2 µm
| Fast
| 43 mJ/cm<sup>2</sup>
| 0
| >2 µm (a lot of stitching)
| Reversal bake: 120s@110°C, Flood exposure: 200mJ/cm<sup>2</sup>, Dev: SP60s
|-style="background:LightGrey; color:black"
| 2021-08-25<br>jehem
| 2.2 µm
| Quality
| 26 mJ/cm<sup>2</sup>
| -4
| 1.75 µm
| Reversal bake: 120s@110°C, Flood exposure: 200mJ/cm<sup>2</sup>, Dev: SP60s
|-


|-
'''Quality control'''<br>
|-style="background:WhiteSmoke; color:black"
Please note that the values listed in the table are <i>'''not'''</i> routinely tested as part of quality control, except for the resist AZ 5214E.
!AZ MiR 701<br><span style="color:red">Old PFOA containing version</span>
| 2021-08-25<br>jehem
| 1.5 µm
| Fast
| 225 mJ/cm<sup>2</sup>  
| -4
| 1.25 µm<br>Tested using dehydration reducing measures
| PEB: 60s@110°C, Dev: SP60s
|-style="background:WhiteSmoke; color:black"
|-


{| class="wikitable"
|-
|-
|-style="background:LightGrey; color:black"
! !! Date !! Operator !! Film thickness !! Exposure mode !! Dose !! Defoc !! Resolution !! Comments
!rowspan="2"| AZ nLOF 2020
| 2020-02-01<br>jehem
| 2.0 µm
| Fast
| 300 mJ/cm<sup>2</sup>
| 0
| 2 µm (due to stitching)
| PEB: 60s@110°C, Dev: SP60s
|-style="background:LightGrey; color:black"
| 2020-03-01<br>taran
| 2.0 µm
| Quality
| 180-200 mJ/cm<sup>2</sup>
| 0
| 1 µm
| PEB: 60s@110°C, Dev: SP60s
|-
|-
 
! scope=row| AZ MIR 701
| 2025-10-16 || jehem || 1.5 µm || Fast || 325 mJ/cm<sup>2</sup> || -1 || 1.5 µm || '''Not under regular quality control'''<br><br>Post exposure bake: 60 s @ 110°C<br>Development: 60 s puddle<br><br>Tested using dehydration reducing measures
|-
|-
|-style="background:WhiteSmoke; color:black"
! scope=row| AZ 5214E
!AZ 5214E<br><span style="color:green">New Japanese version</span>
| 2025-08-15 || taran || 1.5 µm || Fast|| 110 mJ/cm<sup>2</sup> || -1 || 1.75 µm || See QC data for latest values<br><br>Development: 60 s puddle
| 2023-01-06<br>jehem
| 1.5 µm
| Fast
| 80 mJ/cm<sup>2</sup>
| -2
| 1.75 µm
| Dev: SP60s
|-style="background:WhiteSmoke; color:black"
|-
|-
 
! scope=row| AZ 5214E<br>Image reversal
| 2023-04-05 || jehem || 2.2 µm || Fast|| 20 mJ/cm<sup>2</sup><br><span style="color:red">possibly incorrect data</span> || -2<br><span style="color:red">possibly incorrect data</span> || 2.0 µm || '''Not under regular quality control'''<br><br>Reversal bake: 60 s @ 110°C<br>Flood exposure: 500 mJ/cm<sup>2</sup><br>Development: 60 s puddle
|-
|-
|-style="background:LightGrey; color:black"
! scope=row| AZ nLOF 2020
!AZ 5214E image reversal<br><span style="color:green">New Japanese version</span>
| 2023-07-06 || jehem || 2.0 µm || Fast || 180 mJ/cm<sup>2</sup> || 0 || 1.5 µm || '''Not under regular quality control'''<br><br>Post exposure bake: 60 s @ 110°C<br>Development: 60 s puddle
| 2023-01-11<br>jehem
| 2.2 µm
| Fast
| 42 mJ/cm<sup>2</sup>
| -2
| 1.75 µm
| Reversal bake: 60s@110°C, Flood exposure: 500mJ/cm<sup>2</sup>, Dev: SP60s
|-
|-
! scope=row| AZ 4562
| 2023-04-05 || jehem || 10 µm || Fast|| 1050 mJ/cm<sup>2</sup><br><span style="color:red">possibly incorrect data</span> || -1<br><span style="color:red">possibly incorrect data</span> || ≤5 µm || '''Not under regular quality control'''<br><br>Priming: HMDS<BR>Rehydration after SB: none<br>Exposure: Single exposure<br>Degassing after exposure: none<br>Development: 5 x 60 s multi puddle
|}


|-
'''New resists version in 2023'''<br>
|-style="background:WhiteSmoke; color:black"
As of 2023-03-21 we no longer have any of the old versions of the resists: AZ 5214E, AZ 4562, AZ MiR 701. This table contains only information about the new resist versions.
!AZ MiR 701<br><span style="color:green">New PFOA free version</span>
| 2021-08-25<br>jehem
| 1.5 µm
| Fast
| 225 mJ/cm<sup>2</sup>
| -4
| 1.25 µm (due to stitching)<br>Tested using dehydration reducing measures
| PEB: 60s@110°C, Dev: SP60s
|-
 
|-
|-style="background:LightGrey; color:black"
!AZ 4562<br><span style="color:green">New Japanese version</span>
| 2021-12-07<br>jehem
| 10 µm
| Fast
| 750 mJ/cm<sup>2</sup>
| 0
| ≤5 µm
| Priming: HMDS<BR>Rehydration after SB: 1 hour (may not be necessary)<br>Exposure: Multiple exposures with pauses, 5 x (10 s exposure + 10 s pause)<br>Degassing after exposure: 1 hour (may not be necessary)<br>Development: Multiple puddles, 5 x 60 s
|-


|}
<br>
'''Dehydration reducing measures used for testing AZ MiR 701:'''<br>
'''Dehydration reducing measures used for testing AZ MiR 701:'''<br>
The CDA used for the pneumatic autofocus will dehydrate the resist. To reduce this effect, the writehead is parked far away from the write area while setting up the job for at least a few minutes, before starting the exposure.
The CDA used for the pneumatic autofocus will dehydrate the resist. To reduce this effect, the writehead is parked far away from the write area while setting up the job for at least a few minutes, before starting the exposure.
<br clear="all" />


===Aligner: Maskless 02===
===Aligner: Maskless 02===
The Aligner: Maskless 02 has a 375 nm laser light source, and a 405 nm laser light source, each with a FWHM of ~1 nm.
The Aligner: Maskless 02 has a 375 nm laser light source with a FWHM of ~1 nm. The test exposures on this tool were made using the optical autofocus system, unless otherwise specified.


{|border="1" cellspacing="1" cellpadding="7" style="text-align:left;"
'''Quality control'''<br>
|-
Please note that the values listed in the table are <i>'''not'''</i> routinely tested as part of quality control, except for the resist AZ 5214E.


{| class="wikitable"
|-
|-
|-style="background:silver; color:black"
!  !! Date !! Operator !! Film thickness !! Exposure mode !! Dose !! Defoc !! Resolution !! Comments
|
!Date
!Thickness
!Laser
!Exposure mode
!Dose
!Defoc
!Resolution
!Comments
|-
|-
 
! scope=row| AZ MIR 701
| 2023-08-21 || taran || 1.5 µm || Quality || 325 mJ/cm<sup>2</sup> || 1 || 1 µm || '''Not under regular quality control'''<br><br>Post exposure bake: 60 s @ 110°C<br>Development: 60 s puddle<br><br>Tested using dehydration reducing measures
|-
|-
|-style="background:WhiteSmoke; color:black"
! scope=row| AZ 5214E
!rowspan="2"| AZ 5206E<br>(AZ5214E diluted with PGMEA 1:1 per volume)<br><span style="color:red">Old German version</span>
| 2024-12-09 || taran || 1.5 µm || Quality|| 100 mJ/cm<sup>2</sup> || 2 || 1.5 µm || See QC data for latest values<br><br>Development: 60 s puddle
| Long ago
|rowspan="2"| 0.5 µm
|rowspan="2"| 375 nm
| Fast
| 60 mJ/cm<sup>2</sup>
| -6
| 1 µm (not optimized)
| Dev: 2xSP30s
|-style="background:WhiteSmoke; color:black"
| Long ago
| Quality
| 60 mJ/cm<sup>2</sup>
| -6
| ~750 nm (not optimized)
| Dev: 2xSP30s
|-
|-
 
! scope=row| AZ 5214E<br>Image reversal
| 2023-04-17 || jehem || 2.2 µm || Quality|| 35 mJ/cm<sup>2</sup> || 0 || 1.5 µm || '''Not under regular quality control'''<br><br>Reversal bake: 60 s @ 110°C<br>Flood exposure: 500 mJ/cm<sup>2</sup><br>Development: 60 s puddle
|-
|-
|-style="background:LightGrey; color:black"
! scope=row| AZ nLOF 2020
!rowspan="3"| AZ 5214E<br><span style="color:red">Old German version</span>
| 2023-08-21 || taran || 2.0 µm || Quality || 450 mJ/cm<sup>2</sup> || 0 || 1.5 µm || '''Not under regular quality control'''<br><br>Post exposure bake: 60 s @ 110°C<br>Development: 60 s puddle
| Long ago
|rowspan="3"| 1.5 µm
| 405 nm
| Fast
| 90 mJ/cm<sup>2</sup>
| -2
| 1-2 µm
| Dev: SP60s
|-style="background:LightGrey; color:black"
| Long ago
|rowspan="2"| 375 nm
| Fast
| 65 mJ/cm<sup>2</sup>
| 2
| ~1 µm
| Dev: SP60s
|-style="background:LightGrey; color:black"
| Long ago
| Quality
| 65 mJ/cm<sup>2</sup>
| 2
| ~750 nm
| Dev: SP60s
|-
|-
 
! scope=row| AZ 4562
|-
| 2023-04-19 || jehem || 10 µm || Quality|| 1150 mJ/cm<sup>2</sup> || 0 || ≤5 µm || '''Not under regular quality control'''<br><br>Priming: HMDS<BR>Rehydration after SB: none<br>Exposure: Single exposure<br>Degassing after exposure: none<br>Development: 5 x 60 s multi puddle
|-style="background:WhiteSmoke; color:black"
!rowspan="3"| AZ MiR 701<br><span style="color:red">Old PFOA containing version</span>
| Long ago
|rowspan="3"| 1.5 µm
| 405 nm
| Fast
| 200 mJ/cm<sup>2</sup>
| -5
| ~1 µm (not optimized)
| PEB: 60s@110°C, Dev: SP60s
|-style="background:WhiteSmoke; color:black"
| Long ago
|rowspan="2"| 375 nm
| Fast
| 170 mJ/cm<sup>2</sup>
| -5
| 1 µm
| PEB: 60s@110°C, Dev: SP60s
|-style="background:WhiteSmoke; color:black"
| Long ago
| Quality
| 180 mJ/cm<sup>2</sup>
| -6 (Feb 2019) <br> -2 (Apr 2019)
| <750 nm
| PEB: 60s@110°C, Dev: SP60s <br> Large structures probably over-exposed
|-
 
|-
|-style="background:LightGrey; color:black"
!rowspan="2"| AZ nLOF 2020
| 2021-02-22<br>jehem
|rowspan="2"| 2 µm
|rowspan="2"| 375 nm
| Fast
| 350 mJ/cm<sup>2</sup>
| 0
| 1 µm
| PEB: 120s@110°C, Dev: SP60s
|-style="background:LightGrey; color:black"
| 2021-02-22<br>jehem
| Quality
| 350 mJ/cm<sup>2</sup>
| 0
| 1 µm
| PEB: 120s@110°C, Dev: SP60s
|-
 
|}
|}


<br>
'''New writehead'''<br>
As of 2023-03-21 the MLA2 has a new writehead installed, converting it from a write mode 1 tool to a write mode 2 tool. This makes all previous dose/defocus settings obsolete. This table contains only the dose/defocus values for the new writehead.


{|border="1" cellspacing="1" cellpadding="7" style="text-align:left;"
'''New resists version in 2023'''<br>
|-
As of 2023-03-21 we no longer have any of the old versions of the resists: AZ 5214E, AZ 4562, AZ MiR 701. This table contains only information about the new resist versions.


|-
|-style="background:silver; color:black"
|
!Date
!Thickness
!Laser
!Autofocus
!Exposure mode
!Dose
!Defoc
!Resolution
!Comments
|-
|-
|-style="background:WhiteSmoke; color:black"
!AZ 5214E<br><span style="color:green">New Japanese version</span>
| 2021-08-20<br>jehem
| 1.5 µm
| 375
| Optical
| Fast
| 70 mJ/cm<sup>2</sup>
| -4
| 1 µm
| Dev: SP60s
|-style="background:WhiteSmoke; color:black"
|-
|-
|-style="background:LightGrey; color:black"
!AZ 5214E image reversal<br><span style="color:green">New Japanese version</span>
| 2021-11-25<br>jehem
| 2.2 µm
| 375
| Optical
| Fast
| <s>16 mJ/cm<sup>2</sup></s>
| <s>-4</s>
| <s>1.75 µm</s>
| Reversal bake: 60s@110°C, Flood exposure: 500mJ/cm<sup>2</sup>, Dev: SP60s
|-
|-
|-style="background:WhiteSmoke; color:black"
!AZ MiR 701<br><span style="color:green">New PFOA free version</span>
| 2021-08-20<br>jehem
| 1.5 µm
| 375
| Optical
| Fast
| 200 mJ/cm<sup>2</sup>
| -6
| 1 µm<br>Tested using dehydration reducing measures
| PEB: 60s@110°C, Dev: SP60s
|-
|-
|-style="background:LightGrey; color:black"
!AZ 4562<br><span style="color:green">New Japanese version</span>
| 2021-12-08<br>jehem
| 10 µm
| 375
| Optical
| Fast
| 750 mJ/cm<sup>2</sup>
| 0
| ≤5 µm
| Priming: HMDS<BR>Rehydration after SB: 1 hour (may not be necessary)<br>Exposure: Multiple exposures with pauses, 5 x (10 s exposure + 10 s pause)<br>Degassing after exposure: 1 hour (may not be necessary)<br>Development: Multiple puddles, 5 x 60 s
|-
|}
<br>
'''Dehydration reducing measures used for testing AZ MiR 701:'''<br>
'''Dehydration reducing measures used for testing AZ MiR 701:'''<br>
The CDA used for the pneumatic autofocus will dehydrate the resist. To reduce this effect, the writehead is parked far away from the write area while setting up the job for at least a few minutes, before starting the exposure.
The CDA used for the pneumatic autofocus will dehydrate the resist. To reduce this effect, the writehead is parked far away from the write area while setting up the job for at least a few minutes, before starting the exposure.


==Aligner: Maskless 03==
<br clear="all" />
The Aligner: Maskless 03 has a 405 nm laser light source with a FWHM of ~1 nm.


{|border="1" cellspacing="1" cellpadding="7" style="text-align:left;"
===Aligner: Maskless 03===
|-
The Aligner: Maskless 03 has a 405 nm laser light source with a FWHM of ~1 nm. The test exposures on this tool were made using the pneumatic autofocus system.


|-
'''Quality control'''<br>
|-style="background:silver; color:black"
Please note that the values listed in the table are <i>'''not'''</i> routinely tested as part of quality control, except for the resist AZ 5214E.
|
!Date
!Thickness
!Exposure mode
!Dose
!Defoc
!Resolution
!Comments
|-


{| class="wikitable"
|-
|-
|-style="background:WhiteSmoke; color:black"
! !! Date !! Operator !! Film thickness !! Exposure mode !! Dose !! Defoc !! Resolution !! Comments
!rowspan="2"| AZ 5214E<br><span style="color:red">Old German version</span>
| 2020-10-01<br>jehem
|rowspan="2"| 1.5 µm
| Fast
| 70 mJ/cm<sup>2</sup>
| 0
| 2 µm (due to stitching)
| Dev: SP60s
|-style="background:WhiteSmoke; color:black"
| 2021-03-23<br>jehem
| Quality
| 65 mJ/cm<sup>2</sup>
| -2
| 1 µm
| Dev: SP60s
|-
|-
 
! scope=row| AZ MIR 701
| 2025-10-20 || jehem || 1.5 µm || Quality || 175 mJ/cm<sup>2</sup> || -1 || 1 µm || '''Not under regular quality control'''<br><br>Post exposure bake: 60 s @ 110°C<br>Development: 60 s puddle<br><br>Tested using dehydration reducing measures
|-
|-
|-style="background:WhiteSmoke; color:black"
! scope=row| AZ 5214E
!rowspan="2"| AZ MiR 701<br><span style="color:red">Old PFOA containing version</span>
| 2025-09-02 || taran || 1.5 µm || Quality|| 75 mJ/cm<sup>2</sup> || 1 || 1 µm || See QC data for latest values<br><br>Development: 60 s puddle
| 2020-02-01<br>jehem
|rowspan="2"| 1.5 µm
| Fast
| 300 mJ/cm<sup>2</sup>
| 0
| 2 µm (due to stitching)<br>Non optimized dehydration reduction
| PEB: 60s@110°C, Dev: SP60s
|-style="background:WhiteSmoke; color:black"
| 2021-08-25<br>jehem
| Quality
| 175 mJ/cm<sup>2</sup>
| -2
| 1 µm<br>Tested using dehydration reducing measures
| PEB: 60s@110°C, Dev: SP60s
|-
|-
 
! scope=row| AZ 5214E<br>Image reversal
| 2023-06-30 || jehem || 2.2 µm || Quality|| 50 mJ/cm<sup>2</sup> || 0 || 1 µm || '''Not under regular quality control'''<br><br>Reversal bake: 60 s @ 110°C<br>Flood exposure: 500 mJ/cm<sup>2</sup><br>Development: 60 s puddle
|-
|-
|-style="background:WhiteSmoke; color:black"
! scope=row| AZ nLOF 2020
!rowspan="2"| AZ 5214E image reversal<br><span style="color:red">Old German version</span>
| 2023-06-30 || jehem || 2 µm || Quality|| 9000 mJ/cm<sup>2</sup> || 2 || 1 µm || '''Not under regular quality control'''<br><br>Post exposure bake: 60 s @ 110°C<br>Development: 60 s puddle<br><br><span style="color:red">'''Due to the high dose required on this tool, it is recommended to process nLOF on tools with a more appropriate exposure light source'''</span>
| 2020-10-01<br>jehem
|rowspan="2"| 2.2 µm
| Fast
| 43 mJ/cm<sup>2</sup>
| 0
| >2 µm (a lot of stitching)
| Reversal bake: 120s@110°C, Flood exposure: 200mJ/cm<sup>2</sup>, Dev: SP60s
|-style="background:WhiteSmoke; color:black"
| 2021-08-25<br>jehem
| Quality
| 32 mJ/cm<sup>2</sup>
| -1
| 1 µm
| Reversal bake: 120s@110°C, Flood exposure: 200mJ/cm<sup>2</sup>, Dev: SP60s
|-
|-
 
! scope=row| AZ 4562
| 2023-06-30 || jehem || 10 µm || Quality|| 550 mJ/cm<sup>2</sup> || 3 || ≤5 µm || '''Not under regular quality control'''<br><br>Priming: HMDS<BR>Rehydration after SB: none<br>Exposure: Single exposure<br>Degassing after exposure: none<br>Development: 5 x 60 s multi puddle
|}
|}


'''New resists version in 2023'''<br>
As of 2023-03-21 we no longer have any of the old versions of the resists: AZ 5214E, AZ 4562, AZ MiR 701. This table contains only information about the new resist versions.


'''AZ nLOF 2020''' has also been tested. It seems to work even at 405nm, but the dose is so high (>10000) that exposure would be slower than Aligner: Maskless 02.
<br>
<br>
{|border="1" cellspacing="1" cellpadding="7" style="text-align:left;"
|-
|-
|-style="background:silver; color:black"
|
!Date
!Thickness
!Laser
!Autofocus
!Exposure mode
!Dose
!Defoc
!Resolution
!Comments
|-
|-
|-style="background:WhiteSmoke; color:black"
!AZ 5214E<br><span style="color:green">New Japanese version</span>
| 2023-01-06<br>taran
| 1.5 µm
| 405
| Pneumatic
| Quality
| 70 mJ/cm<sup>2</sup>
| -2
| 1 µm
| Dev: SP60s
|-style="background:WhiteSmoke; color:black"
|-
|-
|-style="background:LightGrey; color:black"
!AZ 5214E image reversal<br><span style="color:green">New Japanese version</span>
| 2023-01-06<br>taran
| 2.2 µm
| 405
| Pneumatic
| Quality
| 50 mJ/cm<sup>2</sup>
| -2
| 1 µm
| Reversal bake: 60s@110°C, Flood exposure: 500mJ/cm<sup>2</sup>, Dev: SP60s
|-
|-
|-style="background:WhiteSmoke; color:black"
!AZ MiR 701<br><span style="color:green">New PFOA free version</span>
| 2021-08-25<br>jehem
| 1.5 µm
| 405
| Pneumatic
| Quality
| 175 mJ/cm<sup>2</sup>
| -2
| 1 µm<br>Tested using dehydration reducing measures
| PEB: 60s@110°C, Dev: SP60s
|-
|-
|-style="background:LightGrey; color:black"
!AZ 4562<br><span style="color:green">New Japanese version</span>
| 2021-12-08<br>jehem
| 10 µm
| 405
| Pneumatic
| Quality
| 550 mJ/cm<sup>2</sup>
| 1
| ≤5 µm
| Priming: HMDS<BR>Rehydration after SB: 1 hour (may not be necessary)<br>Exposure: Multiple exposures with pauses, 5 x (10 s exposure + 10 s pause)<br>Degassing after exposure: 1 hour (may not be necessary)<br>Development: Multiple puddles, 5 x 60 s
|-
|}
<br>
'''Dehydration reducing measures used for testing AZ MiR 701:'''<br>
'''Dehydration reducing measures used for testing AZ MiR 701:'''<br>
The CDA used for the pneumatic autofocus will dehydrate the resist. To reduce this effect, the writehead is parked far away from the write area while setting up the job for at least a few minutes, before starting the exposure.
The CDA used for the pneumatic autofocus will dehydrate the resist. To reduce this effect, the writehead is parked far away from the write area while setting up the job for at least a few minutes, before starting the exposure.


=Exposure dose when using AZ 351B developer (NaOH)=
<br clear="all" />
 
==Exposure dose when using AZ 351B developer (NaOH)==
The exposure doses listed below are for ''generic'' good exposure results, and can be a compromise between getting good lines, as well as good dots, in both clear field and dark field exposures. The optimal dose for any given specific project, could be different from the listed values.
The exposure doses listed below are for ''generic'' good exposure results, and can be a compromise between getting good lines, as well as good dots, in both clear field and dark field exposures. The optimal dose for any given specific project, could be different from the listed values.


All doses are for standard silicon wafers, unless otherwise stated. Development is done using AZ 351B developer (NaOH).
All doses are for standard silicon wafers, unless otherwise stated. Development is done using AZ 351B developer (NaOH) diluted 1:5.


==KS Aligner (351B)==
The KS Aligner has an i-line notch filter installed. This results in an exposure light peak around 365 nm with a FWHM of 7 nm.


{|border="1" cellspacing="1" cellpadding="7" style="text-align:left;"
===Aligner: MA6-1===
|-
The Aligner: MA6-1 has an i-line notch filter installed. This produces an exposure light peak around 365 nm with a FWHM of 7 nm.
 
'''Quality control'''<br>
Please note that the values listed in the table are <i>'''not'''</i> routinely tested as part of quality control.


{| class="wikitable"
|-
|-
|-style="background:silver; color:black"
!  !! Date !! Operator !! Film thickness !! Exposure mode !! Dose !! Resolution !! Comments
|
!Date
!Thickness
!Dose
!Development]
!Comments
|-
|-
 
! scope=row| AZ 5214E
| Long ago || ? || 1.5 µm || ? || 70 mJ/cm<sup>2</sup> || ? µm || '''Not under regular quality control'''<br><br>Development: 60 s submersion
|-
|-
|-style="background:WhiteSmoke; color:black"
! scope=row| AZ 5214E
!rowspan="3"|AZ 5214E
| Long ago || ? || 2.2 µm || ? || 72 mJ/cm<sup>2</sup> || ? µm || '''Not under regular quality control'''<br><br>Development: 70 s submersion
|Long ago
|1.5 µm
|70mJ/cm<sup>2</sup>
|60 s
|rowspan="3"|Positive process
|-style="background:WhiteSmoke; color:black"
|Long ago
|2.2 µm
|72 mJ/cm<sup>2</sup>
|70 s
|-style="background:WhiteSmoke; color:black"
|Long ago
|4.2 µm
|160 mJ/cm<sup>2</sup>
|180 s
|-
 
|-
|-
|-style="background:LightGrey; color:black"
! scope=row| AZ 5214E
!rowspan="2"|AZ 5214E
| Long ago || ? || 4.2 µm || ? || 160 mJ/cm<sup>2</sup> || ? µm || '''Not under regular quality control'''<br><br>Development: 180 s submersion
|Long ago
|1.5 µm
|30 mJ/cm<sup>2</sup>
|60 s
|rowspan="2"|Image reversal process.
 
Reversal bake: 100s at 110°C.<br>Flood exposure after reversal bake: 210 mJ/cm<sup>2</sup>
|-style="background:LightGrey; color:black"
|Long ago
|2.2 µm
|35 mJ/cm<sup>2</sup>
|70 s
|-
|-
 
! scope=row| AZ 5214E<br>Image reversal
| Long ago || ? || 1.5 µm || ? || 30 mJ/cm<sup>2</sup> || ? µm || '''Not under regular quality control'''<br><br>Reversal bake: 100 s @ 110°C<br>Flood exposure: 210 mJ/cm<sup>2</sup><br>Development: 60 s submersion
|-
|-
|-style="background:WhiteSmoke; color:black"
! scope=row| AZ 5214E<br>Image reversal
!AZ 4562
| Long ago || ? || 2.2 µm || ? || 35 mJ/cm<sup>2</sup> || ? µm || '''Not under regular quality control'''<br><br>Reversal bake: 100 s @ 110°C<br>Flood exposure: 210 mJ/cm<sup>2</sup><br>Development: 70 s submersion
|Long ago
|10 µm
|320 mJ/cm<sup>2</sup>
|5 minutes
|Multiple exposure with 10-15 s pauses is recommended.
|-
|-
! scope=row| AZ 4562
| Long ago || ? || 10 µm || ? || 320 mJ/cm<sup>2</sup> || ? µm || '''Not under regular quality control'''<br><br>Priming: HMDS<BR>Rehydration after SB: none<br>Exposure: Multiple exposures with 15 s pauses is recommended<br>Degassing after exposure: none<br>Development: 300 s submersion
|}
|}
'''New resists version in 2023'''<br>
As of 2023-03-21 we no longer have any of the old versions of the resists: AZ 5214E, AZ 4562, AZ MiR 701. <span style="color:red">This table contains only information about the <i>old</i> resist versions.</span>
<br clear="all" />

Revision as of 15:00, 20 October 2025

UV resist comparison table

Comparison of specifications and feature space of the standard UV photoresists available at DTU Nanolab.

Resist AZ 5214E AZ MiR 701 AZ nLOF 2020 AZ 4562 SU-8 TI Spray
Resist tone
  • Positive
  • Negative (image reversal)
Positive Negative Positive Negative
  • Positive
  • Negative (image reversal)
Thickness range 1.5 - 4.2 µm 1.5 - 4 µm 1.5 - 4 µm 5 - 10 µm 1 - 200 µm 0.5 - 5 µm
Coating tool

Automatic spin coaters:

  • Spin coater: Gamma UV lithography
  • Spin coater: Gamma E-beam & UV

Manual spin coaters:

  • Spin coater: Labspin 02
  • Spin coater: Labspin 03
  • Spin coater: RCD8

Spray coater

Automatic spin coaters:

  • Spin coater: Gamma UV lithography
  • Spin coater: Gamma E-beam & UV

Manual spin coaters:

  • Spin coater: Labspin 02
  • Spin coater: Labspin 03
  • Spin coater: RCD8

Spray coater

Automatic spin coaters:

  • Spin coater: Gamma UV lithography

Manual spin coaters:

  • Spin coater: Labspin 02
  • Spin coater: Labspin 03
  • Spin coater: RCD8

Spray coater

Automatic spin coaters:

  • Spin coater: Gamma E-beam & UV

Manual spin coaters:

  • Spin coater: Labspin 02
  • Spin coater: Labspin 03
  • Spin coater: RCD8

Manual spin coaters:

  • Spin coater: Labspin 02
  • Spin coater: Labspin 03
  • Spin coater: RCD8

Spray coater

Spectral sensitivity 310 - 420 nm 310 - 445 nm 310 - 380 nm 310 - 445 nm 300 - 375 nm 310 - 440 nm
Exposure tool
  • Maskless aligners
  • Mask aligners
  • Maskless aligners
  • Mask aligners
  • Maskless aligners
  • Mask aligners
  • Maskless aligners
  • Mask aligners
  • Maskless aligners
  • Mask aligners
  • Maskless aligners
  • Mask aligners
Developer
  • AZ 726 MIF (2.38% TMAH)
  • AZ 351 B (NaOH)
  • AZ 726 MIF (2.38% TMAH)
  • AZ 351 B (NaOH)

AZ 726 MIF (2.38% TMAH)

mr-DEV 600 (PGMEA)

AZ 726 MIF (2.38% TMAH)

Development rinse agent DIW DIW DIW DIW IPA DIW
Remover
  • Acetone
  • Remover 1165 (NMP)
  • Acetone
  • Remover 1165 (NMP)
  • Acetone
  • Remover 1165 (NMP)

Remover 1165 (NMP)

  • Cross-linked SU-8 is practically insoluble
  • Oxygen plasma ashing can remove cross-linked SU-8
  • Acetone
  • Remover 1165 (NMP)
Comments Good adhesion for wet etch High selectivity for dry etch Negative sidewalls for lift-off For processes with resist thickness between 6 µm and 25 µm
  • High aspect ratio
  • Resist thickness 1 µm to hundreds of µm
  • Available in cleanroom: 2005, 2035, and 2075. Considering discontinuation of the SU-8 2000 series we need to move to another product SU8 3000 and SU8 XTF series.
  • New formulation will be available in cleanroom and tested: 3005 instead of 2005, 3035 instead of 2035, XTF75 instead of 2075 and new 3025.
TI spray resist is an image reversal resist, similar to AZ 5214E. The process flow will be similar to the process flows for 5214, except for the coating step. The exposure dose and development will depend on the specific process.


Process flow examples

Comparison of specifications and feature space of the standard UV photoresists available at DTU Nanolab. These are just examples and may contain obsolete information regarding exposure dose, etc.

Resist AZ 5214E AZ MIR 701 AZ nLOF 2020 AZ 4562 SU-8 Ti Spray
Maskless aligner

Process flow AZ MiR 701‎ MLA

Process flow AZ nLOF 2020‎ MLA‎

Process flow AZ 4562 MLA

Process flow SU-8 MLA‎

NB! Most of the process knowledge about SU-8 is based in research groups

Mask aligner

Process flow AZ MiR 701‎ MA6

Process flow AZ nLOF 2020‎ MA6‎

Process flow AZ 4562 MA6‎

Process flow SU-8 MA6‎

NB! Most of the process knowledge about SU-8 is based in research groups

Other process flows: Chip on carrier: A procedure for UV lithography on a chip using automatic coater and developer.


Exposure dose

Spectral sensitivity of AZ resists represented as optical absorption coefficient.

During exposure of the resist, the photoinitiator, or photo-active component, reacts with the exposure light, and starts the reaction which makes the resist develop in the developer.

In a positive resist, it makes the resist become soluble in the developer. In a negative resist, usually assisted by thermal energy in the post-exposure bake (PEB), it makes the resist insoluble in the developer. The amount of light required to fully develop the resist in the development process, is the exposure dose.

The optimal exposure dose is a function of many parameters, including the type of resist, the resist thickness, and the sensitivity of the resist.

Resist sensitivity
The resist sensitivity is a measure of how efficiently it reacts to the exposure light. Spectral sensitivity is the sensitivity of the resist as a function of wavelength. It is usually given simply as the range from the wavelength below which absorption in the resist material makes lithography impractical to the wavelength at which the photoinitiator is no longer efficiently activated.

Within the sensitivity range, the optical absorption is commonly used as a measure of sensitivity. A high absorption coefficient signifies a high sensitivity, as the light is absorbed by the photoinitiator. Because of spectral sensitivity, the optimal dose of a given resist type and thickness is also a function of the spectral distribution of the exposure light, i.e. the equipment used for the exposure. Using a combination of experience, calculation and assumptions, it may be possible to estimate the dose for an exposure equipment, if the exposure dose is already known on another equipment.

Due to reflection and refraction at the interface between the resist and the substrate, the optimal dose may also be a function of the type of substrate used. Unless otherwise stated, the exposure doses given below are for standard silicon wafers.

Apart from the already mentioned factors, the optimal dose also depends on the developer chemistry and the parameters used in the development process. Finally, the requirements to the lithographic process in terms of resolution, bias (line broadening), etch selectivity, side wall angle, etc. may narrow down, or widen, the process window. The exposure doses given in the sections below should be used as a starting point for individual fabrication process development.

Due to the process of bleaching, where the absorption of the resist changes during exposure, the exposure dose is unfortunately not always constant at different intensities of the exposure light. The exposure time is thus not always a linear function of the exposure intensity.

Calculate exposure time

In the maskless aligners, the dose is set directly as a process parameter in the job. In mask aligners, on the other hand, the parameter that is set is the exposure time, i.e. how long the shutter is open during the exposure.

The exposure dose, D [J/m2], in terms if exposure light intensity I [W/m2] and exposure time t [s], is given by:

D=It

Since the intensity is specific to the spectral sensitivity of the sensor used to measure the exposure light, and the exposure time is specific to the spectral distribution of the exposure light (cf. spectral sensitivity), this dose is specific to the combination of exposure source and optical sensor.

Given an exposure dose, the exposure time, t, is calculated as:

t=DI1

It is important to keep in mind that this exposure time is valid only for a specific combination of exposure source and optical sensor, as well as for a specific development process.

Exposure dose for mask aligners

The exposure doses listed below are for generic good exposure results, and can be a compromise between getting good lines, as well as good dots, in both clear field and dark field exposures. The optimal dose for any given specific project, could be different from the listed values.

All doses are for standard silicon wafers, unless otherwise stated. Development is done using 2.38% TMAH (AZ 726 MIF).


Aligner: MA6-1

The Aligner: MA6-1 has an i-line notch filter installed. This produces an exposure light peak around 365 nm with a FWHM of 7 nm.

Quality control
Please note that the values listed in the table are not routinely tested as part of quality control.

Date Operator Film thickness Exposure mode Dose Resolution Comments
AZ MIR 701 Long ago ? 1.5 µm ? 180 mJ/cm2 ? µm Not under regular quality control

Post exposure bake: 60 s @ 110°C
Development: 60 s puddle
AZ MIR 701 Long ago ? 2.0 µm ? 200 mJ/cm2 ? µm Not under regular quality control

Post exposure bake: 60 s @ 110°C
Development: 60 s puddle
AZ MIR 701 Long ago ? 4.0 µm ? 400 mJ/cm2 ? µm Not under regular quality control

Post exposure bake: 60 s @ 110°C
Development: 60 s puddle
AZ 5214E Long ago ? 1.5 µm ? 72 mJ/cm2 ? µm Not under regular quality control

Development: 60 s puddle
AZ 5214E Long ago ? 2.2 µm ? 80 mJ/cm2 ? µm Not under regular quality control

Development: 60 s puddle
AZ 5214E Long ago ? 4.2 µm ? 160 mJ/cm2 ? µm Not under regular quality control

Development: 60 s puddle
AZ 5214E
Image reversal
Long ago ? 2.2 µm ? ? mJ/cm2 ? µm Not under regular quality control

Reversal bake: 60 s @ 110°C
Flood exposure: 500 mJ/cm2
Development: 60 s puddle
AZ nLOF 2020 Long ago ? 2.0 µm ? 121 mJ/cm2 ? µm Not under regular quality control

Post exposure bake: 60 s @ 110°C
Development: 60 s puddle

Side wall angle: ~15°
For smaller angle (~5°): develop 30 seconds instead
AZ 4562 Long ago ? 10 µm ? 510 mJ/cm2 ≤5 µm Not under regular quality control

Priming: HMDS
Rehydration after SB: none
Exposure: Multiple exposures with 15 s pauses is recommended
Degassing after exposure: none
Development: 5 x 60 s multi puddle

New resists version in 2023
As of 2023-03-21 we no longer have any of the old versions of the resists: AZ 5214E, AZ 4562, AZ MiR 701. This table contains only information about the old resist versions.


Aligner: MA6-2

The Aligner: MA6-2 has an i-line notch filter installed. This produces an exposure light peak around 365 nm with a FWHM of 7 nm.

Quality control
Please note that the values listed in the table are not routinely tested as part of quality control.

Date Operator Film thickness Exposure mode Dose Resolution Comments
AZ MIR 701 2023-09-26 taran 1.5 µm Hard contact 150 mJ/cm2 ? µm Not under regular quality control

Post exposure bake: 60 s @ 110°C
Development: 60 s puddle
AZ 5214E 2025-09-30 jehem 1.5 µm Hard contact 90 mJ/cm2 1.5 µm Not under regular quality control

Development: 60 s puddle
AZ 5214E
Image reversal
2023-01-11 jehem 2.2 µm Hard contact 22 mJ/cm2 2.0 µm Not under regular quality control

Reversal bake: 60 s @ 110°C
Flood exposure: 500 mJ/cm2
Development: 60 s puddle
AZ nLOF 2020 2023-09-26 taran 2.0 µm Hard contact 121 mJ/cm2 ? µm Not under regular quality control

Post exposure bake: 60 s @ 110°C
Development: 60 s puddle
AZ 4562 2021-12-08 jehem 10 µm Soft contact 550 mJ/cm2 ≤5 µm Not under regular quality control

Priming: HMDS
Rehydration after SB: none
Exposure: Single exposure
Degassing after exposure: none
Development: 5 x 60 s multi puddle

New resists version in 2023
As of 2023-03-21 we no longer have any of the old versions of the resists: AZ 5214E, AZ 4562, AZ MiR 701. This table contains only information about the new resist versions.


Exposure dose for maskless aligners

The exposure doses listed below are for generic good exposure results, and can be a compromise between getting good lines, as well as good dots, in both clear field and dark field exposures. The optimal dose and achievable resolution for any given specific project, could be different from the listed values.

All doses are for standard silicon wafers, unless otherwise stated. Development is done using 2.38% TMAH (AZ 726 MIF).


Aligner: Maskless 01

The Aligner: Maskless 01 has a 365 nm laser light source with a FWHM of ~1 nm. The test exposures on this tool were made using the pneumatic autofocus system.

Quality control
Please note that the values listed in the table are not routinely tested as part of quality control, except for the resist AZ 5214E.

Date Operator Film thickness Exposure mode Dose Defoc Resolution Comments
AZ MIR 701 2025-10-16 jehem 1.5 µm Fast 325 mJ/cm2 -1 1.5 µm Not under regular quality control

Post exposure bake: 60 s @ 110°C
Development: 60 s puddle

Tested using dehydration reducing measures
AZ 5214E 2025-08-15 taran 1.5 µm Fast 110 mJ/cm2 -1 1.75 µm See QC data for latest values

Development: 60 s puddle
AZ 5214E
Image reversal
2023-04-05 jehem 2.2 µm Fast 20 mJ/cm2
possibly incorrect data
-2
possibly incorrect data
2.0 µm Not under regular quality control

Reversal bake: 60 s @ 110°C
Flood exposure: 500 mJ/cm2
Development: 60 s puddle
AZ nLOF 2020 2023-07-06 jehem 2.0 µm Fast 180 mJ/cm2 0 1.5 µm Not under regular quality control

Post exposure bake: 60 s @ 110°C
Development: 60 s puddle
AZ 4562 2023-04-05 jehem 10 µm Fast 1050 mJ/cm2
possibly incorrect data
-1
possibly incorrect data
≤5 µm Not under regular quality control

Priming: HMDS
Rehydration after SB: none
Exposure: Single exposure
Degassing after exposure: none
Development: 5 x 60 s multi puddle

New resists version in 2023
As of 2023-03-21 we no longer have any of the old versions of the resists: AZ 5214E, AZ 4562, AZ MiR 701. This table contains only information about the new resist versions.

Dehydration reducing measures used for testing AZ MiR 701:
The CDA used for the pneumatic autofocus will dehydrate the resist. To reduce this effect, the writehead is parked far away from the write area while setting up the job for at least a few minutes, before starting the exposure.


Aligner: Maskless 02

The Aligner: Maskless 02 has a 375 nm laser light source with a FWHM of ~1 nm. The test exposures on this tool were made using the optical autofocus system, unless otherwise specified.

Quality control
Please note that the values listed in the table are not routinely tested as part of quality control, except for the resist AZ 5214E.

Date Operator Film thickness Exposure mode Dose Defoc Resolution Comments
AZ MIR 701 2023-08-21 taran 1.5 µm Quality 325 mJ/cm2 1 1 µm Not under regular quality control

Post exposure bake: 60 s @ 110°C
Development: 60 s puddle

Tested using dehydration reducing measures
AZ 5214E 2024-12-09 taran 1.5 µm Quality 100 mJ/cm2 2 1.5 µm See QC data for latest values

Development: 60 s puddle
AZ 5214E
Image reversal
2023-04-17 jehem 2.2 µm Quality 35 mJ/cm2 0 1.5 µm Not under regular quality control

Reversal bake: 60 s @ 110°C
Flood exposure: 500 mJ/cm2
Development: 60 s puddle
AZ nLOF 2020 2023-08-21 taran 2.0 µm Quality 450 mJ/cm2 0 1.5 µm Not under regular quality control

Post exposure bake: 60 s @ 110°C
Development: 60 s puddle
AZ 4562 2023-04-19 jehem 10 µm Quality 1150 mJ/cm2 0 ≤5 µm Not under regular quality control

Priming: HMDS
Rehydration after SB: none
Exposure: Single exposure
Degassing after exposure: none
Development: 5 x 60 s multi puddle

New writehead
As of 2023-03-21 the MLA2 has a new writehead installed, converting it from a write mode 1 tool to a write mode 2 tool. This makes all previous dose/defocus settings obsolete. This table contains only the dose/defocus values for the new writehead.

New resists version in 2023
As of 2023-03-21 we no longer have any of the old versions of the resists: AZ 5214E, AZ 4562, AZ MiR 701. This table contains only information about the new resist versions.

Dehydration reducing measures used for testing AZ MiR 701:
The CDA used for the pneumatic autofocus will dehydrate the resist. To reduce this effect, the writehead is parked far away from the write area while setting up the job for at least a few minutes, before starting the exposure.


Aligner: Maskless 03

The Aligner: Maskless 03 has a 405 nm laser light source with a FWHM of ~1 nm. The test exposures on this tool were made using the pneumatic autofocus system.

Quality control
Please note that the values listed in the table are not routinely tested as part of quality control, except for the resist AZ 5214E.

Date Operator Film thickness Exposure mode Dose Defoc Resolution Comments
AZ MIR 701 2025-10-20 jehem 1.5 µm Quality 175 mJ/cm2 -1 1 µm Not under regular quality control

Post exposure bake: 60 s @ 110°C
Development: 60 s puddle

Tested using dehydration reducing measures
AZ 5214E 2025-09-02 taran 1.5 µm Quality 75 mJ/cm2 1 1 µm See QC data for latest values

Development: 60 s puddle
AZ 5214E
Image reversal
2023-06-30 jehem 2.2 µm Quality 50 mJ/cm2 0 1 µm Not under regular quality control

Reversal bake: 60 s @ 110°C
Flood exposure: 500 mJ/cm2
Development: 60 s puddle
AZ nLOF 2020 2023-06-30 jehem 2 µm Quality 9000 mJ/cm2 2 1 µm Not under regular quality control

Post exposure bake: 60 s @ 110°C
Development: 60 s puddle

Due to the high dose required on this tool, it is recommended to process nLOF on tools with a more appropriate exposure light source
AZ 4562 2023-06-30 jehem 10 µm Quality 550 mJ/cm2 3 ≤5 µm Not under regular quality control

Priming: HMDS
Rehydration after SB: none
Exposure: Single exposure
Degassing after exposure: none
Development: 5 x 60 s multi puddle

New resists version in 2023
As of 2023-03-21 we no longer have any of the old versions of the resists: AZ 5214E, AZ 4562, AZ MiR 701. This table contains only information about the new resist versions.

Dehydration reducing measures used for testing AZ MiR 701:
The CDA used for the pneumatic autofocus will dehydrate the resist. To reduce this effect, the writehead is parked far away from the write area while setting up the job for at least a few minutes, before starting the exposure.


Exposure dose when using AZ 351B developer (NaOH)

The exposure doses listed below are for generic good exposure results, and can be a compromise between getting good lines, as well as good dots, in both clear field and dark field exposures. The optimal dose for any given specific project, could be different from the listed values.

All doses are for standard silicon wafers, unless otherwise stated. Development is done using AZ 351B developer (NaOH) diluted 1:5.


Aligner: MA6-1

The Aligner: MA6-1 has an i-line notch filter installed. This produces an exposure light peak around 365 nm with a FWHM of 7 nm.

Quality control
Please note that the values listed in the table are not routinely tested as part of quality control.

Date Operator Film thickness Exposure mode Dose Resolution Comments
AZ 5214E Long ago ? 1.5 µm ? 70 mJ/cm2 ? µm Not under regular quality control

Development: 60 s submersion
AZ 5214E Long ago ? 2.2 µm ? 72 mJ/cm2 ? µm Not under regular quality control

Development: 70 s submersion
AZ 5214E Long ago ? 4.2 µm ? 160 mJ/cm2 ? µm Not under regular quality control

Development: 180 s submersion
AZ 5214E
Image reversal
Long ago ? 1.5 µm ? 30 mJ/cm2 ? µm Not under regular quality control

Reversal bake: 100 s @ 110°C
Flood exposure: 210 mJ/cm2
Development: 60 s submersion
AZ 5214E
Image reversal
Long ago ? 2.2 µm ? 35 mJ/cm2 ? µm Not under regular quality control

Reversal bake: 100 s @ 110°C
Flood exposure: 210 mJ/cm2
Development: 70 s submersion
AZ 4562 Long ago ? 10 µm ? 320 mJ/cm2 ? µm Not under regular quality control

Priming: HMDS
Rehydration after SB: none
Exposure: Multiple exposures with 15 s pauses is recommended
Degassing after exposure: none
Development: 300 s submersion

New resists version in 2023
As of 2023-03-21 we no longer have any of the old versions of the resists: AZ 5214E, AZ 4562, AZ MiR 701. This table contains only information about the old resist versions.