Jump to content

Specific Process Knowledge/Lithography/Resist/UVresist: Difference between revisions

From LabAdviser
Jehem (talk | contribs)
Taran (talk | contribs)
(47 intermediate revisions by 3 users not shown)
Line 84: Line 84:
Manual coaters:<br>
Manual coaters:<br>
*Spin coater: RCD8
*Spin coater: RCD8
or
*Spin coater: Labspin 2
*Spin coater: Labspin 3
|
|
Spray coater
Spray coater
Line 102: Line 105:
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
!Exposure tool
!Exposure tool
|align="center" colspan="5"|Mask aligner or Maskless aligner
|align="center" colspan="6"|Mask aligner or Maskless aligner
|-
|-


Line 114: Line 117:
*AZ 351B
*AZ 351B
*AZ 726 MIF
*AZ 726 MIF
|AZ 726 MIF
|
*AZ 726 MIF
*[[Specific_Process_Knowledge/Lithography/nLOF#Development|Solvent development]] possible
|AZ 726 MIF
|AZ 726 MIF
|mr-DEV 600 (PGMEA)
|mr-DEV 600 (PGMEA)
Line 169: Line 174:
*High aspect ratio
*High aspect ratio
*Resist thickness 1 µm to several 100 µm
*Resist thickness 1 µm to several 100 µm
*Available in cleanroom: 2005, 2035, and 2075. Considering discontinuation of the SU-8 2000 series we need to move to another product SU8 3000 and SU8 XTF series.
*New formulation will be available in cleanroom and tested: 3005 instead of 2005, 3035 instead of 2035, XTF75 instead of 2075 and new 3025.
|
|
Spray coater specific resist
Spray coater specific resist
Line 229: Line 236:


==Exposure dose==
==Exposure dose==
[[Image:AZ photoresists spectral sensitivity - remake v1.png|400x400px|thumb|Spectral sensitivity of AZ resists represented as optical absorption coefficient.]]
[[Image:resistSensitivity_UV.png|400px|thumb|Spectral sensitivity of AZ resists represented as optical absorption coefficient.]]


During exposure of the resist, the photoinitiator, or photo-active component, reacts with the exposure light, and starts the reaction which makes the resist develop in the developer.
During exposure of the resist, the photoinitiator, or photo-active component, reacts with the exposure light, and starts the reaction which makes the resist develop in the developer.
Line 266: Line 273:
The exposure doses listed below are for ''generic'' good exposure results, and can be a compromise between getting good lines, as well as good dots, in both clear field and dark field exposures. The optimal dose for any given specific project, could be different from the listed values.
The exposure doses listed below are for ''generic'' good exposure results, and can be a compromise between getting good lines, as well as good dots, in both clear field and dark field exposures. The optimal dose for any given specific project, could be different from the listed values.


All doses are for standard silicon wafers, unless otherwise stated. Development is done using 2.38% TMAH.
All doses are for standard silicon wafers, unless otherwise stated. Development is done using 2.38% TMAH (AZ 726 MIF).




===KS Aligner===
===Aligner: MA6-1===
The KS Aligner has an i-line notch filter installed. This results in an exposure light peak around 365 nm with a FWHM of 7 nm.
The Aligner: MA6-1 has an i-line notch filter installed. This results in an exposure light peak around 365 nm with a FWHM of 7 nm.


{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
Line 287: Line 294:
|-
|-
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
!rowspan="3"|AZ 5214E<br><span style="color:red">Old German version</span>
!rowspan="3"|AZ 5214E<br><span style="color:red">Data from discontinued German version</span>
|Long ago
|Long ago
|1.5 µm
|1.5 µm
Line 305: Line 312:
|-
|-
|-style="background:LightGrey; color:black"
|-style="background:LightGrey; color:black"
!AZ 4562<br><span style="color:red">Old German version</span>
!AZ 4562<br><span style="color:red">Data from discontinued German version</span>
|Long ago
|Long ago
|10 µm
|10 µm
Line 315: Line 322:
|-
|-
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
!rowspan="3"|AZ MiR 701<br><span style="color:red">Old PFOA containing version</span>
!rowspan="3"|AZ MiR 701<br><span style="color:red">Data from discontinued PFOA containing version</span>
|Long ago
|Long ago
|1 µm
|1 µm
Line 348: Line 355:




===Aligner: MA6 - 2===
===Aligner: MA6-2===
The Aligner: MA6-2 has an i-line notch filter installed. This results in an exposure light peak around 365 nm with a FWHM of 7 nm.
The Aligner: MA6-2 has an i-line notch filter installed. This results in an exposure light peak around 365 nm with a FWHM of 7 nm.
'''New resists'''<br>
As of 2023-03-21 we no longer have any of the old versions of the resists: AZ 5214E, AZ 4562, AZ MiR 701. The following table contains only information about the new resist versions.


{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
Line 365: Line 375:


|-
|-
|-style="background:WhiteSmoke; color:black"
|-style="background:whitesmoke; color:black"
!rowspan="2"|AZ 5214E<br><span style="color:red">Old German version</span>
!AZ MiR 701
|Long ago
|2023-09-26<br>taran
|1.5 µm
|1.5 µm
|72 mJ/cm<sup>2</sup>
|150 mJ/cm<sup>2</sup>
|Single puddle, 60 s
(13.5s @ 11mW/cm<sup>2</sup>)
|rowspan="2"|Positive process
|-style="background:WhiteSmoke; color:black"
|Long ago
|2.2 µm
|90 mJ/cm<sup>2</sup>
|Single puddle, 60 s
|Single puddle, 60 s
|PEB: 60 s @ 110°C
|-
|-


|-
|-
|-style="background:LightGrey; color:black"
|-style="background:silver; color:black"
!rowspan="2"|AZ 5214E Image Reversal<br><span style="color:red">Old German version</span>
!AZ nLOF 2020
|Long ago
|2023-09-26<br>taran
|1.5 µm
|22 mJ/cm<sup>2</sup>
|Single puddle, 60 s
|rowspan="2"|Image reversal process.<br>Reversal bake: 120 s at 110°C.<br>Flood exposure: 200 mJ/cm<sup>2</sup>
|-style="background:LightGrey; color:black"
|Long ago
|2.2 µm
|25 mJ/cm<sup>2</sup>
|Single puddle, 60 s
|-
 
|-
|-style="background:WhiteSmoke; color:black"
!rowspan="3"|AZ MiR 701<br><span style="color:red">Old PFOA containing version</span>
|Long ago
|1.5 µm
|169 mJ/cm<sup>2</sup>
|Single puddle, 60 s
|rowspan="2"|PEB: 60 s at 110°C
|-style="background:WhiteSmoke; color:black"
|Long ago
|2 µm
|2 µm
|200 mJ/cm<sup>2</sup>
|121 mJ/cm<sup>2</sup>
(11 s @ 11 mW/cm<sup>2</sup>)
|Single puddle, 60 s
|Single puddle, 60 s
|-style="background:WhiteSmoke; color:black"
|PEB: 60 s @ 110°C<br>60 s development for lift-off
|Long ago
|4 µm
|280 mJ/cm<sup>2</sup>
|Single puddle, 60 s
|rowspan="1"|PEB: 60 s at 110°C<br>Process adopted from process logs
|-
 
|-
|-style="background:LightGrey; color:black"
!AZ nLOF 2020
|Long ago
|1.5 µm
|104 mJ/cm<sup>2</sup>
|Single puddle, 30 s
|PEB: 60 s at 110°C<br>Use 60 s development for lift-off
|-
|-


|-
|-
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
!AZ 5214E<br><span style="color:green">New Japanese version</span>
!AZ 5214E
|2023-01-11<br>jehem
|2023-01-11<br>jehem
|1.5 µm
|1.5 µm
Line 436: Line 407:


|-
|-
|-style="background:LightGrey; color:black"
|-style="background:silver; color:black"
!AZ 5214E Image Reversal<br><span style="color:green">New Japanese version</span>
!AZ 5214E<br>Image Reversal
|2023-01-11<br>jehem
|2023-01-11<br>jehem
|2.2 µm
|2.2 µm
|22 mJ/cm<sup>2</sup>
|22 mJ/cm<sup>2</sup>
|Single puddle, 60 s
|Single puddle, 60 s
|Image reversal process.<br>Reversal bake: 60 s at 110°C.<br>Flood exposure: 500 mJ/cm<sup>2</sup>
|
Reversal bake: 60 s at 110°C<br>
Flood exposure: 500 mJ/cm<sup>2</sup>
|-
|-


|-
|-
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
!AZ 4562<br><span style="color:green">New Japanese version</span>
!AZ 4562<br>
|2021-12-08<br>jehem
|2021-12-08<br>jehem
|10 µm
|10 µm
|550 mJ/cm<sup>2</sup>
|550 mJ/cm<sup>2</sup>
|Multiple puddles, 5 x 60 s
|Multiple puddles, 5 x 60 s
|Priming: HMDS<BR>Rehydration after SB: 1 hour (may not be necessary)<br>Exposure: Multiple exposures with pauses, 5 x (10 s exposure + 10 s pause)<br>Degassing after exposure: 1 hour (may not be necessary)
|
|-
Priming: HMDS<BR>
 
Rehydration after SB: 1 hour (may not be necessary)<br>
|-
Exposure: Multiple exposures with pauses, 5 x (10 s exposure + 10 s pause)<br>
|-style="background:LightGrey; color:black"
Degassing after exposure: 1 hour (may not be necessary)
!AZ MiR 701<br><span style="color:green">New PFOA free version</span>
|2021-06-23<br>elkh
|1.5 µm
|150 mJ/cm<sup>2</sup>
|Single puddle, 60 s
|PEB: 60 s at 110°C
|-
|-
|}
|}
Line 468: Line 435:


==Exposure dose for maskless aligners==
==Exposure dose for maskless aligners==
The exposure doses listed below are for ''generic'' good exposure results, and can be a compromise between getting good lines, as well as good dots, in both clear field and dark field exposures. The optimal dose for any given specific project, could be different from the listed values.
The exposure doses listed below are for ''generic'' good exposure results, and can be a compromise between getting good lines, as well as good dots, in both clear field and dark field exposures. The optimal dose and achievable resolution for any given specific project, could be different from the listed values.


All doses are for standard silicon wafers, unless otherwise stated. Development is done using 2.38% TMAH.
All doses are for standard silicon wafers, unless otherwise stated. Development is done using 2.38% TMAH (AZ 726 MIF).




Line 496: Line 463:
|-
|-
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
!AZ MiR 701<br>jehem
!AZ MiR 701
| 2023-04-04
| 2023-07-06<br>jehem
| 1.5 µm
| 1.5 µm
| Fast
| Fast
| 305 mJ/cm<sup>2</sup>
| 275 mJ/cm<sup>2</sup>
| 0
| 1
| 1.25 µm<br>Tested using dehydration reducing measures
| 1 µm<br>Tested using dehydration reducing measures
| PEB: 60s@110°C<br>Dev: SP60s
| PEB: 60s@110°C<br>Dev: SP60s
|-
|-
Line 509: Line 476:
|-style="background:silver; color:black"
|-style="background:silver; color:black"
!AZ nLOF 2020
!AZ nLOF 2020
| 2023-04-04
| 2023-07-06<br>jehem
| 2.0 µm
| 2.0 µm
| Fast
| Fast
| 160 mJ/cm<sup>2</sup>
| 180 mJ/cm<sup>2</sup>
| -3
| 0
| 1.5 µm
| 1.5 µm
| PEB: 60s@110°C<br>Dev: SP60s
| PEB: 60s@110°C<br>Dev: SP60s
Line 521: Line 488:
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
!AZ 5214E
!AZ 5214E
| 2023-04-04
| 2024-11-29<br>taran
| 1.5 µm
| 1.5 µm
| Fast
| Fast
| 95 mJ/cm<sup>2</sup>
| 105 mJ/cm<sup>2</sup>
| -3
| 3
| 2.0 µm
| 1.75 µm
| Dev: SP60s
| Dev: SP60s
|-
|-
Line 533: Line 500:
|-style="background:silver; color:black"
|-style="background:silver; color:black"
!AZ 5214E<br>image reversal
!AZ 5214E<br>image reversal
| 2023-04-04
| <span style="color:red">2023-04-05</span><br>jehem
| 2.2 µm
| 2.2 µm
| Fast
| Fast
| 20 mJ/cm<sup>2</sup>
| <span style="color:red">possibly obsolete data</span><br>20 mJ/cm<sup>2</sup>
| -2
| <span style="color:red">possibly obsolete data</span><br>-2
| 2.0 µm
| 2.0 µm
| Reversal bake: 60s@110°C,<br>Flood exposure: 500mJ/cm<sup>2</sup><br>Dev: SP60s  
| Reversal bake: 60s@110°C,<br>Flood exposure: 500mJ/cm<sup>2</sup><br>Dev: SP60s  
Line 545: Line 512:
|-style="background:whitesmoke; color:black"
|-style="background:whitesmoke; color:black"
!AZ 4562
!AZ 4562
| Not tested yet
| <span style="color:red">2023-04-05</span><br>jehem
| 10 µm
| 10 µm
| Fast
| Fast
|  
| <span style="color:red">possibly obsolete data</span><br>1050 mJ/cm<sup>2</sup>
|  
| <span style="color:red">possibly obsolete data</span><br>-1
|  
| ≤5 µm
|  
|  
Priming: HMDS<BR>
Priming: HMDS<BR>
Line 596: Line 563:
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
!rowspan="2"| AZ MiR 701
!rowspan="2"| AZ MiR 701
|rowspan="2"| 2023-03-21<br>jehem
|rowspan="2"| 2023-08-21 <br> taran
|rowspan="2"| 1.5 µm
|rowspan="2"| 1.5 µm
|rowspan="2"| 375
|rowspan="2"| 375
| Optical
| Optical
|rowspan="2"| Quality
|rowspan="2"| Quality
|rowspan="2"| 415 mJ/cm<sup>2</sup>
|rowspan="2"| 325 mJ/cm<sup>2</sup>
| 6
| 1
|rowspan="2"| 1 µm<br>Tested using dehydration reducing measures
|rowspan="2"| 1 µm<br>Tested using dehydration reducing measures<br>(design elongated +40mm in y).
|rowspan="2"|  
|rowspan="2"|  
PEB: 60s @ 110°C<br>
PEB: 60s @ 110°C<br>
Line 609: Line 576:
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
| Pneumatic
| Pneumatic
| 2
| ?
|-
|-


Line 615: Line 582:
|-style="background:silver; color:black"
|-style="background:silver; color:black"
!rowspan="2"| AZ nLOF 2020
!rowspan="2"| AZ nLOF 2020
|rowspan="2"| 2023-03-21<br>jehem
|rowspan="2"| 2023-08-21 <br> taran
|rowspan="2"| 2.0 µm
|rowspan="2"| 2.0 µm
|rowspan="2"| 375
|rowspan="2"| 375
| Optical
| Optical
|rowspan="2"| Quality
|rowspan="2"| Quality
|rowspan="2"| 700 mJ/cm<sup>2</sup>
|rowspan="2"| 450 mJ/cm<sup>2</sup>
| 6
| 0
|rowspan="2"| 1.5 µm
|rowspan="2"| 1.5 µm
|rowspan="2"|
|rowspan="2"|
Line 628: Line 595:
|-style="background:silver; color:black"
|-style="background:silver; color:black"
| Pneumatic
| Pneumatic
| 2
| ?
|-
|-


Line 634: Line 601:
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
!rowspan="2"| AZ 5214E
!rowspan="2"| AZ 5214E
|rowspan="2"| 2023-03-21<br>jehem
|rowspan="2"| 2024-12-09<br>taran
|rowspan="2"| 1.5 µm
|rowspan="2"| 1.25 µm
|rowspan="2"| 375
|rowspan="2"| 375
| Optical
| Optical
|rowspan="2"| Quality
|rowspan="2"| Quality
|rowspan="2"| 120 mJ/cm<sup>2</sup>
|rowspan="2"| 100 mJ/cm<sup>2</sup>
| 6
| 2
|rowspan="2"| 1 µm
|rowspan="2"| 1.5 µm
|rowspan="2"| Dev: SP60s
|rowspan="2"| Dev: SP60s
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
| Pneumatic
| Pneumatic
| 2
| -2 (?)
|-
|-


Line 651: Line 618:
|-style="background:silver; color:black"
|-style="background:silver; color:black"
!rowspan="2"| AZ 5214E<br>image reversal
!rowspan="2"| AZ 5214E<br>image reversal
|rowspan="2"| 2023-03-21<br>jehem
|rowspan="2"| 2023-04-17 <br> jehem
|rowspan="2"| 2.2 µm
|rowspan="2"| 2.2 µm
|rowspan="2"| 375
|rowspan="2"| 375
| Optical
| Optical
|rowspan="2"| Quality
|rowspan="2"| Quality
|rowspan="2"| 45 mJ/cm<sup>2</sup>
|rowspan="2"| 35 mJ/cm<sup>2</sup>
| 6
| 0
|rowspan="2"| 1.5 µm
|rowspan="2"| 1.5 µm
|rowspan="2"|  
|rowspan="2"|  
Line 665: Line 632:
|-style="background:silver; color:black"
|-style="background:silver; color:black"
| Pneumatic
| Pneumatic
| 2
| ?
|-
|-


Line 671: Line 638:
|-style="background:whitesmoke; color:black"
|-style="background:whitesmoke; color:black"
!rowspan="2"| AZ 4562
!rowspan="2"| AZ 4562
|rowspan="2"| Not tested yet
|rowspan="2"| 2023-04-19<br>jehem
|rowspan="2"| 10 µm
|rowspan="2"| 10 µm
|rowspan="2"| 375
|rowspan="2"| 375
| Optical
| Optical
|rowspan="2"| Quality
|rowspan="2"| Quality
|rowspan="2"| 1150 mJ/cm<sup>2</sup>
| 0
|rowspan="2"| ≤5 µm
|rowspan="2"|  
|rowspan="2"|  
|
|rowspan="2"|
|rowspan="2"|
Priming: HMDS<br>
Priming: HMDS<br>
Rehydration after softbake: 1 hour (may not be necessary)<br>
Rehydration after softbake: 1 hour (may not be necessary)<br>
Line 687: Line 654:
|-style="background:whitesmoke; color:black"
|-style="background:whitesmoke; color:black"
| Pneumatic
| Pneumatic
|  
| ?
|-
|-


Line 699: Line 666:
===Aligner: Maskless 03===
===Aligner: Maskless 03===
The Aligner: Maskless 03 has a 405 nm laser light source with a FWHM of ~1 nm.
The Aligner: Maskless 03 has a 405 nm laser light source with a FWHM of ~1 nm.
'''New resists'''<br>
As of 2023-03-21 we no longer have any of the old versions of the resists: AZ 5214E, AZ 4562, AZ MiR 701. The following table contains only information about the new resist versions.


{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
Line 719: Line 689:
|-
|-
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
!rowspan="2"| AZ 5214E<br><span style="color:red">Old German version</span>
!AZ MiR 701
| 2020-10-01
| 2023-06-30<br>jehem
|rowspan="2"| 1.5 µm
| 1.5 µm
| 405 nm
| 405
| Pneumatic
| Fast
| 70 mJ/cm<sup>2</sup>
| 0
| 2 µm (due to stitching)
| Dev: SP60s
 
|-style="background:WhiteSmoke; color:black"
| 2021-03-23
| 405 nm
| Pneumatic
| Pneumatic
| Quality
| Quality
| 65 mJ/cm<sup>2</sup>
| 175 mJ/cm<sup>2</sup>
| -2
| 1 µm
| Dev: SP60s
|-
 
|-
|-style="background:silver; color:black"
!rowspan="2"| AZ MiR 701<br><span style="color:red">Old PFOA containing version</span>
| 2020-02-01
|rowspan="2"| 1.5 µm
| 405 nm
| Pneumatic
| Fast
| 300 mJ/cm<sup>2</sup>
| 0
| 0
| 2 µm (due to stitching)<br>Non optimized dehydration reduction
| PEB: 60s@110°C, Dev: SP60s
|-style="background:silver; color:black"
| 2021-08-25
| 405 nm
| Pneumatic
| Quality
| 175 mJ/cm<sup>2</sup>
| -2
| 1 µm<br>Tested using dehydration reducing measures
| 1 µm<br>Tested using dehydration reducing measures
| PEB: 60s@110°C, Dev: SP60s
| PEB: 60s@110°C<br>Dev: SP60s
|-
|-


|-
|-
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
!rowspan="2"| AZ 5214E image reversal<br><span style="color:red">Old German version</span>
!AZ 5214E
| 2020-10-01
| 2023-06-30<br>jehem
|rowspan="2"| 2.2 µm
| 1.5 µm
| 405 nm
| Pneumatic
| Fast
| 43 mJ/cm<sup>2</sup>
| 0
| >2 µm (a lot of stitching)
| Reversal bake: 120s@110°C, Flood exposure: 200mJ/cm<sup>2</sup>, Dev: SP60s
 
|-style="background:WhiteSmoke; color:black"
| 2021-08-25
| 405 nm
| Pneumatic
| Quality
| 32 mJ/cm<sup>2</sup>
| -1
| 1 µm
| Reversal bake: 120s@110°C, Flood exposure: 200mJ/cm<sup>2</sup>, Dev: SP60s
|-
 
|-
|-style="background:silver; color:black"
!AZ nLOF 2020
| 2023-01-13
| 2.0 µm
| 405
| 405
| Pneumatic
| Pneumatic
| Quality
| Quality
| 9000 mJ/cm<sup>2</sup>
| 75 mJ/cm<sup>2</sup>
| 0
| 0
| 1 µm
| PEB: 60s @ 100°C,<br>Dev: SP60s<br> '''Due to the high dose required on this tool, it is recommended to process nLOF on tools with a more appropriate exposure light source'''
|-
|-
|-style="background:WhiteSmoke; color:black"
!AZ 5214E<br><span style="color:green">New Japanese version</span>
| 2023-01-06
| 1.5 µm
| 405
| Pneumatic
| Quality
| 70 mJ/cm<sup>2</sup>
| -2
| 1 µm
| 1 µm
| Dev: SP60s
| Dev: SP60s
Line 819: Line 717:
|-
|-
|-style="background:silver; color:black"
|-style="background:silver; color:black"
!AZ 5214E image reversal<br><span style="color:green">New Japanese version</span>
!AZ 5214E<br>Image reversal
| 2023-01-06
| 2023-06-30<br>jehem
| 2.2 µm
| 2.2 µm
| 405
| 405
Line 826: Line 724:
| Quality
| Quality
| 50 mJ/cm<sup>2</sup>
| 50 mJ/cm<sup>2</sup>
| -2
| 0
| 1 µm
| 1 µm
| Reversal bake: 60s@110°C, Flood exposure: 500mJ/cm<sup>2</sup>, Dev: SP60s  
|  
Reversal bake: 60s@110°C<br>
Flood exposure: 500mJ/cm<sup>2</sup><br>
Dev: SP60s  
|-
|-


|-
|-
|-style="background:WhiteSmoke; color:black"
|-style="background:silver; color:black"
!AZ MiR 701<br><span style="color:green">New PFOA free version</span>
!AZ nLOF 2020
| 2021-08-25
| 2023-06-30<br>jehem
| 1.5 µm
| 2.0 µm
| 405
| 405
| Pneumatic
| Pneumatic
| Quality
| Quality
| 175 mJ/cm<sup>2</sup>
| 9000 mJ/cm<sup>2</sup>
| -2
| 2
| 1 µm<br>Tested using dehydration reducing measures
| 1 µm
| PEB: 60s@110°C, Dev: SP60s
|  
PEB: 60s @ 100°C<br>
Dev: SP60s<br>
<span style="color:red">'''Due to the high dose required on this tool, it is recommended to process nLOF on tools with a more appropriate exposure light source'''</span>
|-
|-


|-
|-
|-style="background:silver; color:black"
|-style="background:whitesmoke; color:black"
!AZ 4562<br><span style="color:green">New Japanese version</span>
!AZ 4562
| 2021-12-08
| 2023-06-30<br>jehem
| 10 µm
| 10 µm
| 405
| 405
Line 854: Line 758:
| Quality
| Quality
| 550 mJ/cm<sup>2</sup>
| 550 mJ/cm<sup>2</sup>
| 1
| 3
| ≤5 µm
| ≤5 µm
|  
|  
Line 874: Line 778:
The exposure doses listed below are for ''generic'' good exposure results, and can be a compromise between getting good lines, as well as good dots, in both clear field and dark field exposures. The optimal dose for any given specific project, could be different from the listed values.
The exposure doses listed below are for ''generic'' good exposure results, and can be a compromise between getting good lines, as well as good dots, in both clear field and dark field exposures. The optimal dose for any given specific project, could be different from the listed values.


All doses are for standard silicon wafers, unless otherwise stated. Development is done using AZ 351B developer (NaOH).
All doses are for standard silicon wafers, unless otherwise stated. Development is done using AZ 351B developer (NaOH) diluted 1:5.


===KS Aligner (351B)===
 
The KS Aligner has an i-line notch filter installed. This results in an exposure light peak around 365 nm with a FWHM of 7 nm.
===Aligner: MA6-1===
The Aligner: MA6-1 has an i-line notch filter installed. This results in an exposure light peak around 365 nm with a FWHM of 7 nm.


{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
Line 894: Line 799:
|-
|-
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
!rowspan="3"|AZ 5214E
!rowspan="3"|AZ 5214E<br><span style="color:red">Data from discontinued German version</span>
|Long ago
|Long ago
|1.5 µm
|1.5 µm
Line 914: Line 819:
|-
|-
|-style="background:LightGrey; color:black"
|-style="background:LightGrey; color:black"
!rowspan="2"|AZ 5214E
!rowspan="2"|AZ 5214E<br><span style="color:red">Data from discontinued German version</span>
|Long ago
|Long ago
|1.5 µm
|1.5 µm
Line 931: Line 836:
|-
|-
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
!AZ 4562
!AZ 4562<br><span style="color:red">Data from discontinued German version</span>
|Long ago
|Long ago
|10 µm
|10 µm

Revision as of 11:52, 9 April 2025

UV resist comparison table

Comparison of specifications and feature space of UV photoresists.

Resist AZ 5214E AZ MiR 701 AZ nLOF 2020 AZ 4562 SU-8 TI Spray
Resist tone
  • Positive
  • Negative (image reversal)
Positive Negative Positive Negative
  • Positive
  • Negative (image reversal)
Thickness range 1.5 - 4.2 µm 1.5 - 4 µm 1.5 - 4 µm 5 - 10 µm 1 - 200 µm 0.5 - 5 µm
Coating tool

Automatic coaters:

  • Spin coater: Gamma UV lithography
  • Spin coater: Gamma ebeam & UV

Manual coaters:

  • Spin coater: Labspin 2
  • Spin coater: Labspin 3
  • Spin coater: RCD8
  • Spray coater

Automatic coaters:

  • Spin coater: Gamma UV lithography
  • Spin coater: Gamma ebeam & UV

Manual coaters:

  • Spin coater: Labspin 2
  • Spin coater: Labspin 3
  • Spin coater: RCD8
  • Spray coater

Automatic coaters:

  • Spin coater: Gamma UV lithography

Manual coaters:

  • Spin coater: Labspin 2
  • Spin coater: Labspin 3
  • Spin coater: RCD8
  • Spray coater

Automatic coaters:

  • Spin coater: Gamma ebeam & UV

Manual coaters:

  • Spin coater: Labspin 2
  • Spin coater: Labspin 3
  • Spin coater: RCD8

Manual coaters:

  • Spin coater: RCD8

or

  • Spin coater: Labspin 2
  • Spin coater: Labspin 3

Spray coater

Spectral sensitivity 310 - 420 nm 310 - 445 nm 310 - 380 nm 310 - 445 nm 300 - 375 nm 310 - 440 nm
Exposure tool Mask aligner or Maskless aligner
Developer
  • AZ 351B
  • AZ 726 MIF
  • AZ 351B
  • AZ 726 MIF
AZ 726 MIF mr-DEV 600 (PGMEA) AZ 726 MIF
Rinse DIW DIW DIW DIW IPA DIW
Remover
  • Acetone
  • Remover 1165
  • Acetone
  • Remover 1165
  • Acetone
  • Remover 1165

Remover 1165

Cured SU-8 is practically insoluble

Plasma ashing can remove crosslinked SU-8

  • Acetone
  • Remover 1165
Comments
  • Can be used for both positive and image reversed (negative) processes with resist thickness between 1 and 4 µm.
  • Good adhesion for wet etch.

High selectivity for dry etch

Negative sidewalls for lift-off

For processes with resist thickness between 6 µm and 25 µm

  • High aspect ratio
  • Resist thickness 1 µm to several 100 µm
  • Available in cleanroom: 2005, 2035, and 2075. Considering discontinuation of the SU-8 2000 series we need to move to another product SU8 3000 and SU8 XTF series.
  • New formulation will be available in cleanroom and tested: 3005 instead of 2005, 3035 instead of 2035, XTF75 instead of 2075 and new 3025.

Spray coater specific resist

Process flow examples

Mask aligner:
Process flow AZ 5214E positive‎ MA6
Process flow AZ 5214E image reversal MA6


Maskless aligner:
Process flow AZ 5214E positive‎ MLA
Process flow AZ 5214E image reversal MLA

Mask aligner:
Process flow AZ MiR 701‎ MA6


Maskless aligner:
Process flow AZ MiR 701‎ MLA

Mask aligner:
Process flow AZ nLOF 2020‎ MA6‎


Maskless aligner:
Process flow AZ nLOF 2020‎ MLA‎

Mask aligner:
Process flow AZ 4562 MA6‎


Maskless aligner:
Process flow AZ 4562 MLA

Mask aligner:
Process flow SU-8 MA6‎


Maskless aligner:
Process flow SU-8 MLA‎


NB! Most of the process knowledge on SU-8 is based in research groups

TI spray resist is an image reversal resist, similar to AZ 5214E. The process flow will be similar to the process flows for 5214, except for the coating step. The exposure dose and development will depend on the specific process.


Other process flows:

Chip on carrier: A procedure for UV lithography on a chip using automatic coater and developer.

Exposure dose

Spectral sensitivity of AZ resists represented as optical absorption coefficient.

During exposure of the resist, the photoinitiator, or photo-active component, reacts with the exposure light, and starts the reaction which makes the resist develop in the developer.

In a positive resist, it makes the resist become soluble in the developer. In a negative resist, usually assisted by thermal energy in the post-exposure bake (PEB), it makes the resist insoluble in the developer. The amount of light required to fully develop the resist in the development process, is the exposure dose.

The optimal exposure dose is a function of many parameters, including the type of resist, the resist thickness, and the sensitivity of the resist.

Resist sensitivity
The resist sensitivity is a measure of how efficiently it reacts to the exposure light. Spectral sensitivity is the sensitivity of the resist as a function of wavelength. It is usually given simply as the range from the wavelength below which absorption in the resist material makes lithography impractical to the wavelength at which the photoinitiator is no longer efficiently activated.

Within the sensitivity range, the optical absorption is commonly used as a measure of sensitivity. A high absorption coefficient signifies a high sensitivity, as the light is absorbed by the photoinitiator. Because of spectral sensitivity, the optimal dose of a given resist type and thickness is also a function of the spectral distribution of the exposure light, i.e. the equipment used for the exposure. Using a combination of experience, calculation and assumptions, it may be possible to estimate the dose for an exposure equipment, if the exposure dose is already known on another equipment.

Due to reflection and refraction at the interface between the resist and the substrate, the optimal dose may also be a function of the type of substrate used. Unless otherwise stated, the exposure doses given below are for standard silicon wafers.

Apart from the already mentioned factors, the optimal dose also depends on the developer chemistry and the parameters used in the development process. Finally, the requirements to the lithographic process in terms of resolution, bias (line broadening), etch selectivity, side wall angle, etc. may narrow down, or widen, the process window. The exposure doses given in the sections below should be used as a starting point for individual fabrication process development.

Due to the process of bleaching, where the absorption of the resist changes during exposure, the exposure dose is unfortunately not always constant at different intensities of the exposure light. The exposure time is thus not always a linear function of the exposure intensity.

Calculate exposure time

In the maskless aligners, the dose is set directly as a process parameter in the job. In mask aligners, on the other hand, the parameter that is set is the exposure time, i.e. how long the shutter is open during the exposure.

The exposure dose, D [J/m2], in terms if exposure light intensity I [W/m2] and exposure time t [s], is given by:

D=It

Since the intensity is specific to the spectral sensitivity of the sensor used to measure the exposure light, and the exposure time is specific to the spectral distribution of the exposure light (cf. spectral sensitivity), this dose is specific to the combination of exposure source and optical sensor.

Given an exposure dose, the exposure time, t, is calculated as:

t=DI1

It is important to keep in mind that this exposure time is valid only for a specific combination of exposure source and optical sensor, as well as for a specific development process.

Exposure dose for mask aligners

The exposure doses listed below are for generic good exposure results, and can be a compromise between getting good lines, as well as good dots, in both clear field and dark field exposures. The optimal dose for any given specific project, could be different from the listed values.

All doses are for standard silicon wafers, unless otherwise stated. Development is done using 2.38% TMAH (AZ 726 MIF).


Aligner: MA6-1

The Aligner: MA6-1 has an i-line notch filter installed. This results in an exposure light peak around 365 nm with a FWHM of 7 nm.

Date Thickness Dose Development Comments
AZ 5214E
Data from discontinued German version
Long ago 1.5 µm 72 mJ/cm2 Single puddle, 60 s Positive process
Long ago 2.2 µm 80 mJ/cm2
Long ago 4.2 µm 160 mJ/cm2
AZ 4562
Data from discontinued German version
Long ago 10 µm 510 mJ/cm2 Multiple puddle, 4 x 60 s Multiple exposure with 10-15 s pauses is recommended.
AZ MiR 701
Data from discontinued PFOA containing version
Long ago 1 µm 180 mJ/cm2 Single puddle, 60 s PEB: 60 s at 110°C
Long ago 2 µm 200 mJ/cm2 Single puddle, 60 s
Long ago 4 µm 400 mJ/cm2 Single puddle, 60 s PEB: 90 s at 110°C
AZ nLOF 2020 Long ago 2 µm 110 mJ/cm2 Single puddle, 60 s PEB: 60 s at 110°C

Side wall angle ~15°

For smaller angle (~5°), develop 30 seconds instead


Aligner: MA6-2

The Aligner: MA6-2 has an i-line notch filter installed. This results in an exposure light peak around 365 nm with a FWHM of 7 nm.

New resists
As of 2023-03-21 we no longer have any of the old versions of the resists: AZ 5214E, AZ 4562, AZ MiR 701. The following table contains only information about the new resist versions.

Date Thickness Dose Development Comments
AZ MiR 701 2023-09-26
taran
1.5 µm 150 mJ/cm2

(13.5s @ 11mW/cm2)

Single puddle, 60 s PEB: 60 s @ 110°C
AZ nLOF 2020 2023-09-26
taran
2 µm 121 mJ/cm2

(11 s @ 11 mW/cm2)

Single puddle, 60 s PEB: 60 s @ 110°C
60 s development for lift-off
AZ 5214E 2023-01-11
jehem
1.5 µm 70 mJ/cm2 Single puddle, 60 s
AZ 5214E
Image Reversal
2023-01-11
jehem
2.2 µm 22 mJ/cm2 Single puddle, 60 s

Reversal bake: 60 s at 110°C
Flood exposure: 500 mJ/cm2

AZ 4562
2021-12-08
jehem
10 µm 550 mJ/cm2 Multiple puddles, 5 x 60 s

Priming: HMDS
Rehydration after SB: 1 hour (may not be necessary)
Exposure: Multiple exposures with pauses, 5 x (10 s exposure + 10 s pause)
Degassing after exposure: 1 hour (may not be necessary)


Exposure dose for maskless aligners

The exposure doses listed below are for generic good exposure results, and can be a compromise between getting good lines, as well as good dots, in both clear field and dark field exposures. The optimal dose and achievable resolution for any given specific project, could be different from the listed values.

All doses are for standard silicon wafers, unless otherwise stated. Development is done using 2.38% TMAH (AZ 726 MIF).


Aligner: Maskless 01

The Aligner: Maskless 01 has a 365 nm LED light source with a FWHM of 8 nm.

New resists
As of 2023-03-21 we no longer have any of the old versions of the resists: AZ 5214E, AZ 4562, AZ MiR 701. The following table contains only information about the new resist versions.

Date Thickness Exposure mode Dose Defoc Resolution Comments
AZ MiR 701 2023-07-06
jehem
1.5 µm Fast 275 mJ/cm2 1 1 µm
Tested using dehydration reducing measures
PEB: 60s@110°C
Dev: SP60s
AZ nLOF 2020 2023-07-06
jehem
2.0 µm Fast 180 mJ/cm2 0 1.5 µm PEB: 60s@110°C
Dev: SP60s
AZ 5214E 2024-11-29
taran
1.5 µm Fast 105 mJ/cm2 3 1.75 µm Dev: SP60s
AZ 5214E
image reversal
2023-04-05
jehem
2.2 µm Fast possibly obsolete data
20 mJ/cm2
possibly obsolete data
-2
2.0 µm Reversal bake: 60s@110°C,
Flood exposure: 500mJ/cm2
Dev: SP60s
AZ 4562 2023-04-05
jehem
10 µm Fast possibly obsolete data
1050 mJ/cm2
possibly obsolete data
-1
≤5 µm

Priming: HMDS
Rehydration after SB: 1 hour (may not be necessary)
Exposure: Single exposure
Degassing after exposure: 1 hour (may not be necessary)
Development: Multiple puddles, 5 x 60 s


Dehydration reducing measures used for testing AZ MiR 701:
The CDA used for the pneumatic autofocus will dehydrate the resist. To reduce this effect, the writehead is parked far away from the write area while setting up the job for at least a few minutes, before starting the exposure.


Aligner: Maskless 02

The Aligner: Maskless 02 has a 375 nm laser light source with a FWHM of ~1 nm.

New resists
As of 2023-03-21 we no longer have any of the old versions of the resists: AZ 5214E, AZ 4562, AZ MiR 701. The following table contains only information about the new resist versions.

New writehead
As of 2023-03-21 the MLA2 has a new writehead installed, converting it from a write mode 1 tool to a write mode 2 tool. This makes all previous dose/defocus settings obsolete. The following table contains only the dose/defocus values for the new writehead.

Date Thickness Laser Autofocus Exposure mode Dose Defoc Resolution Comments
AZ MiR 701 2023-08-21
taran
1.5 µm 375 Optical Quality 325 mJ/cm2 1 1 µm
Tested using dehydration reducing measures
(design elongated +40mm in y).

PEB: 60s @ 110°C
Dev: SP60s

Pneumatic ?
AZ nLOF 2020 2023-08-21
taran
2.0 µm 375 Optical Quality 450 mJ/cm2 0 1.5 µm

PEB: 60s @ 110°C
Dev: SP60s

Pneumatic ?
AZ 5214E 2024-12-09
taran
1.25 µm 375 Optical Quality 100 mJ/cm2 2 1.5 µm Dev: SP60s
Pneumatic -2 (?)
AZ 5214E
image reversal
2023-04-17
jehem
2.2 µm 375 Optical Quality 35 mJ/cm2 0 1.5 µm

Reversal bake: 60s @ 110°C
Flood exposure: 500 mJ/cm2
Dev: SP60s

Pneumatic ?
AZ 4562 2023-04-19
jehem
10 µm 375 Optical Quality 1150 mJ/cm2 0 ≤5 µm

Priming: HMDS
Rehydration after softbake: 1 hour (may not be necessary)
Exposure: Single exposure
Degassing after exposure: 1 hour (may not be necessary)
Development: Multiple puddles, 5 x 60 s

Pneumatic ?


Dehydration reducing measures used for testing AZ MiR 701:
The CDA used for the pneumatic autofocus will dehydrate the resist. To reduce this effect, the writehead is parked far away from the write area while setting up the job for at least a few minutes, before starting the exposure.


Aligner: Maskless 03

The Aligner: Maskless 03 has a 405 nm laser light source with a FWHM of ~1 nm.

New resists
As of 2023-03-21 we no longer have any of the old versions of the resists: AZ 5214E, AZ 4562, AZ MiR 701. The following table contains only information about the new resist versions.

Date Thickness Laser Autofocus Exposure mode Dose Defoc Resolution Comments
AZ MiR 701 2023-06-30
jehem
1.5 µm 405 Pneumatic Quality 175 mJ/cm2 0 1 µm
Tested using dehydration reducing measures
PEB: 60s@110°C
Dev: SP60s
AZ 5214E 2023-06-30
jehem
1.5 µm 405 Pneumatic Quality 75 mJ/cm2 0 1 µm Dev: SP60s
AZ 5214E
Image reversal
2023-06-30
jehem
2.2 µm 405 Pneumatic Quality 50 mJ/cm2 0 1 µm

Reversal bake: 60s@110°C
Flood exposure: 500mJ/cm2
Dev: SP60s

AZ nLOF 2020 2023-06-30
jehem
2.0 µm 405 Pneumatic Quality 9000 mJ/cm2 2 1 µm

PEB: 60s @ 100°C
Dev: SP60s
Due to the high dose required on this tool, it is recommended to process nLOF on tools with a more appropriate exposure light source

AZ 4562 2023-06-30
jehem
10 µm 405 Pneumatic Quality 550 mJ/cm2 3 ≤5 µm

Priming: HMDS
Rehydration after SB: 1 hour (may not be necessary)
Exposure: Single exposure
Degassing after exposure: 1 hour (may not be necessary)
Development: Multiple puddles, 5 x 60 s


Dehydration reducing measures used for testing AZ MiR 701:
The CDA used for the pneumatic autofocus will dehydrate the resist. To reduce this effect, the writehead is parked far away from the write area while setting up the job for at least a few minutes, before starting the exposure.


Exposure dose when using AZ 351B developer (NaOH)

The exposure doses listed below are for generic good exposure results, and can be a compromise between getting good lines, as well as good dots, in both clear field and dark field exposures. The optimal dose for any given specific project, could be different from the listed values.

All doses are for standard silicon wafers, unless otherwise stated. Development is done using AZ 351B developer (NaOH) diluted 1:5.


Aligner: MA6-1

The Aligner: MA6-1 has an i-line notch filter installed. This results in an exposure light peak around 365 nm with a FWHM of 7 nm.

Date Thickness Dose Development] Comments
AZ 5214E
Data from discontinued German version
Long ago 1.5 µm 70mJ/cm2 60 s Positive process
Long ago 2.2 µm 72 mJ/cm2 70 s
Long ago 4.2 µm 160 mJ/cm2 180 s
AZ 5214E
Data from discontinued German version
Long ago 1.5 µm 30 mJ/cm2 60 s Image reversal process.

Reversal bake: 100s at 110°C.
Flood exposure after reversal bake: 210 mJ/cm2

Long ago 2.2 µm 35 mJ/cm2 70 s
AZ 4562
Data from discontinued German version
Long ago 10 µm 320 mJ/cm2 5 minutes Multiple exposure with 10-15 s pauses is recommended.