Specific Process Knowledge/Thin film deposition/Deposition of Silicon Oxide/Deposition of Silicon Oxide using PECVD: Difference between revisions
| (132 intermediate revisions by 6 users not shown) | |||
| Line 1: | Line 1: | ||
At the moment | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Silicon_Oxide/Deposition_of_Silicon_Oxide_using_PECVD click here]'''<br> | ||
{{CC-bghe1}} | |||
At the moment DTU Nanolab has 2 PECVDs that can deposit silicon oxide with or without dopants of boron, phosphorus. PECVD1 and PECVD2 has been decommissioned and now we have PECVD3 and PECVD4. PECVD3 are for silicon based processing allowing wafers with small amount of metal (<5% wafer coverage). PECVD4 is for clean wafers both for silicon based materials and for III-V materials. Look at the [[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]] page to learn more about the PECVDs at Nanolab. All though PECVD4 and PECVD3 are very much alike you cannot count on that a recipe on one system will give exactly the same results on the other system. | |||
== Deposition of SiO2 with PECVD4 == | |||
{| border="1" cellspacing="2" cellpadding="2" colspan="3" | |||
|bgcolor="#98FB98" |'''Quality Control (QC) for PECVD4 - oxide ''' | |||
|- | |||
| | |||
*[http://labmanager.dtu.dk/d4Show.php?id=5093&mach=395 The QC procedure for PECVD4 - requires login]<br> | |||
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=395 The newest QC data for PECVD4 - requires login] | |||
{| {{table}} | |||
| align="center" | | |||
{| border="1" cellspacing="1" cellpadding="2" align="center" style="width:200px" | |||
! QC Recipe: | |||
! QCOXYD2 | |||
|- | |||
| SiH<sub>4</sub> flow | |||
|12 sccm | |||
|- | |||
|N<sub>2</sub>O flow | |||
|1420 sccm | |||
|- | |||
|N<sub>2</sub> flow | |||
|392 sccm | |||
|- | |||
|Pressure | |||
|550 mTorr | |||
|- | |||
|RF-power | |||
|60 W | |||
|- | |||
|} | |||
| align="center" valign="top"| | |||
{| border="2" cellspacing="1" cellpadding="2" align="center" style="width:500px" | |||
!QC limits | |||
!PECVD4 - OXIDE | |||
|- | |||
|Deposition rate | |||
|70 - 85 nm/min | |||
|- | |||
|Non-uniformity | |||
|<3.0 | |||
|- | |||
|Refractive index | |||
|1.474 - 1.486 | |||
|- | |||
|} | |||
|- | |||
|} | |||
|} | |||
{| border="1" cellspacing="2" cellpadding="2" | |||
|-style="background:Black; color:White" | |||
!|Recipe | |||
!|Dep. rate [nm/min] | |||
!|RI | |||
!|Unif. [%] | |||
!|Stress [MPa] | |||
!|Comments | |||
!|SiH4 [sccm] | |||
!|N2O [sccm] | |||
!|N2 [sccm] | |||
!|B2H6 | |||
!|PH3 | |||
!|Pressure [mTorr] | |||
!|Power [W] | |||
!|Load | |||
!|Tune | |||
!|Time [mm:ss] | |||
!|Tested | |||
|- | |||
|LF SiO<!-- Recipe --> | |||
|75-78 nm/min<!-- Dep. rate [nm/min] --> | |||
|1.480-1.483<!-- RI --> | |||
|± 2.1-2.7%<!-- Unif. [%] --> | |||
|compressive 309 MPa <!-- Stress [MPa] --> | |||
|[[/LF_SiO2 results|Click for more results]]<!-- Comments --> | |||
|12<!-- SiH4 [sccm] --> | |||
|1420<!-- N2O [sccm] --> | |||
|392<!-- N2 [sccm] --> | |||
|<!-- B2H6 --> | |||
|<!-- PH3 --> | |||
|550 mTorr<!-- Pressure [mTorr] --> | |||
|60LF"<!-- Power [W] --> | |||
|<!-- Load --> | |||
|<!-- Tune --> | |||
|1:15/13:00(stress)<!-- Time [mm:ss] --> | |||
|February 2017 bghe<!--Tested --> | |||
|- | |||
|HF SiO<!-- Recipe --> | |||
|63-64 nm/min<!-- Dep. rate [nm/min] --> | |||
|1.476-1.477<!-- RI --> | |||
|± 0.3-0.5%<!-- Unif. [%] --> | |||
|Compressive: 250.5 MPa<!-- Stress [MPa] --> | |||
|[[/HF_SiO2 results|Click for more results]]<!-- Comments --> | |||
|10<!-- SiH4 [sccm] --> | |||
|1420<!-- N2O [sccm] --> | |||
|392<!-- N2 [sccm] --> | |||
|<!-- B2H6 --> | |||
|<!-- PH3 --> | |||
|900 mTorr<!-- Pressure [mTorr] --> | |||
|30HF<!-- Power [W] --> | |||
|<!-- Load --> | |||
|<!-- Tune --> | |||
|2:00/16:00(stress)<!-- Time [mm:ss] --> | |||
|February 2017 bghe<!--Tested --> | |||
|- | |||
|waveguide <!-- Recipe --> | |||
|159.5 nm/min<!-- Dep. rate [nm/min] --> | |||
|1.462<!-- RI --> | |||
|± 0.8%<!-- Unif. [%] --> | |||
|Compressive: 121.9 MPa<!-- Stress [MPa] --> | |||
|<!-- Comments --> | |||
|17<!-- SiH4 [sccm] --> | |||
|2000<!-- N2O [sccm] --> | |||
|<!-- N2 [sccm] --> | |||
|<!-- B2H6 --> | |||
|<!-- PH3 --> | |||
|300 mTorr<!-- Pressure [mTorr] --> | |||
|700 LF<!-- Power [W] --> | |||
|<!-- Load --> | |||
|<!-- Tune --> | |||
|40:00<!-- Time [mm:ss] --> | |||
|February 2017 bghe<!--Tested --> | |||
|- | |||
|BPSG<!-- Recipe --> | |||
|259 nm/min<!-- Dep. rate [nm/min] --> | |||
|1.4593<!-- RI --> | |||
|± 1.7%<!-- Unif. [%] --> | |||
|Compressive: 36.7 MPa<!-- Stress [MPa] --> | |||
|Measured after anneal in Clad1000<!-- Comments --> | |||
|17<!-- SiH4 [sccm] --> | |||
|1600<!-- N2O [sccm] --> | |||
|<!-- N2 [sccm] --> | |||
|135<!-- B2H6 --> | |||
|40<!-- PH3 --> | |||
|900 mTorr<!-- Pressure [mTorr] --> | |||
|800 LF <!-- Power [W] --> | |||
|<!-- Load --> | |||
|<!-- Tune --> | |||
|10:00/56:00(stress)<!-- Time [mm:ss] --> | |||
|February 2017 bghe <!--Tested --> | |||
|- | |||
|BPSG low stress<!-- Recipe --> | |||
|302 nm/min<!-- Dep. rate [nm/min] --> | |||
|1.4598<!-- RI --> | |||
|± 1.7%<!-- Unif. [%] --> | |||
|Compressive: 1.4 MPa<!-- Stress [MPa] --> | |||
|Measured after anneal in Clad1000 <!-- Comments --> | |||
|17<!-- SiH4 [sccm] --> | |||
|1600<!-- N2O [sccm] --> | |||
|<!-- N2 [sccm] --> | |||
|240<!-- B2H6 --> | |||
|60<!-- PH3 --> | |||
|500 mTorr<!-- Pressure [mTorr] --> | |||
|800LF<!-- Power [W] --> | |||
|<!-- Load --> | |||
|<!-- Tune --> | |||
|10:00 <!-- Time [mm:ss] --> | |||
|February 2017 bghe <!--Tested --> | |||
|- | |||
|} | |||
*[[/conformity|SEM images of the conformity of the layer on a structured surface]] | |||
<br clear="all" /> | |||
=Recipes on PECVD3 for deposition of silicon oxides= | |||
{| border="1" cellspacing="2" cellpadding="2" colspan="3" | |||
|bgcolor="#98FB98" |'''Quality Control (QC) for PECVD3 - oxide''' | |||
|- | |||
| | |||
*[http://labmanager.dtu.dk/d4Show.php?id=1402&mach=106 The QC procedure for PECVD3 - requires login]<br> | |||
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=106 The newest QC data for PECVD3 - requires login] | |||
{| {{table}} | |||
| align="center" | | |||
{| border="1" cellspacing="1" cellpadding="2" align="center" style="width:200px" | |||
! QC Recipe: | |||
! QCOXYD2 | |||
|- | |||
| SiH<sub>4</sub> flow | |||
|12 sccm | |||
|- | |||
|N<sub>2</sub>O flow | |||
|1420 sccm | |||
|- | |||
|N<sub>2</sub> flow | |||
|392 sccm | |||
|- | |||
|Pressure | |||
|700 mTorr | |||
|- | |||
|RF-power | |||
|150 W | |||
|- | |||
|} | |||
| align="center" valign="top"| | |||
{| border="2" cellspacing="1" cellpadding="2" align="center" style="width:500px" | |||
!QC limits | |||
!PECVD3 - OXIDE | |||
|- | |||
|Deposition rate | |||
|97 - 112 nm/min | |||
|- | |||
|Non-uniformity | |||
|<2.0 | |||
|- | |||
|Refractive index | |||
|1.467 - 1.474 | |||
|- | |||
|} | |||
|- | |||
|} | |||
|} | |||
===Recipes=== | ===Recipes=== | ||
{| border="1" cellspacing="0" cellpadding="7" | {| border="1" cellspacing="0" cellpadding="7" | ||
| Line 7: | Line 230: | ||
|Recipe name | |Recipe name | ||
|SiH4 flow [sccm] | |SiH4 flow [sccm] | ||
|N< | |N<sub>2</sub>O flow [sccm] | ||
|N2 flow [sccm] | |N2 flow [sccm] | ||
|B2H6 flow [sccm] | |||
|PH3 flow [sccm] | |||
|Pressure [mTorr] | |||
|Power [W] | |||
|Description | |||
|- | |||
|LFSiO2 | |||
|12 | |||
|1420 | |||
|392 | |||
|0 | |||
|0 | |||
|700 | |||
|150 | |||
|New QC implemented in April 2016 | |||
|- | |||
|LFSiO | |||
|12 | |||
|1420 | |||
|392 | |||
|0 | |||
|0 | |||
|550 | |||
|60 | |||
|Uniform silicon oxide | |||
|- | |||
|1PBSG | |||
|17 | |||
|1600 | |||
|0 | |||
|135 | |||
|40 | |||
|500 | |||
|800 LF | |||
|BPSG glass for waveguide cladding layer | |||
|} | |||
LF=Low Frequency | |||
===Expected results=== | |||
{| border="1" cellspacing="0" cellpadding="5" | |||
|- | |||
|Recipe name | |||
|Deposition rate [nm/min] | |||
|RI | |||
|Uniformity [%] | |||
|Stress | |||
|Comment | |||
|- | |||
|LFSiO2 | |||
|105nm/min | |||
|1.47 | |||
|~1.5% | |||
|'''400-402 MPa''' compressive stress '' by Anders Simonsen @nbi.ku.dk April 2016'' | |||
|We have seen that this recipe does not deposit the first minute | |||
|- | |||
|LFSiO | |||
|~75 | |||
|~1.48 | |||
|<1 | |||
|not measured | |||
|. | |||
|- | |||
|1PBSG | |||
|~228 nm/min | |||
|. | |||
|~17% | |||
|not measured | |||
|. | |||
|} | |||
<br clear="all" /> | |||
=Recipes on PECVD3 for deposition of doped oxide= | |||
===Recipes=== | |||
{| border="1" cellspacing="0" cellpadding="7" | |||
|- | |||
|Recipe name | |||
|SiH<sub>4</sub> flow [sccm] | |||
|N<sub>2</sub>O flow [sccm] | |||
|N<sub>2</sub> flow [sccm] | |||
|GeH<sub>4</sub> flow [sccm] (scaled by 100) | |||
|B<sub>2</sub>H<sub>6</sub> flow [sccm] | |||
|PH<sub>3</sub> flow [sccm] | |||
|Pressure [mTorr] | |Pressure [mTorr] | ||
|Power [W] | |Power [W] | ||
|Description | |Description | ||
|- | |- | ||
| | |Core-Ge (not possible anymore as we have no Germanium) | ||
|17 | |17 | ||
|1600 | |1600 | ||
|300 | |||
|300 | |||
|0 | |||
|0 | |0 | ||
|400 | |400 | ||
| | |600 LF | ||
| | |Process for germanium doped core layer developed by Haiyan Ou from DTU Photonics | ||
Annnealing: Anneal bond furnace, recipe "core1100" | |||
|- | |- | ||
|Top-BPSG | |||
|17 | |||
|1600 | |||
|0 | |||
|0 | |||
|100 | |||
|40 | |||
|500 | |||
|800 LF | |||
|Process for PBSG top clading layer developed by Haiyan Ou from DTU Photonics | |||
Annnealing/oxidation: Anneal bond furnace, recipe "clad1000" | |||
|} | |} | ||
| Line 28: | Line 348: | ||
|Recipe name | |Recipe name | ||
|Deposition rate [nm/min] | |Deposition rate [nm/min] | ||
| | |Refractive index | ||
| | |- | ||
|Core-Ge | |||
|~188 nm/min | |||
|~1.46969 | |||
|- | |||
|Top-BPSG | |||
|~248 nm/min | |||
|~1.458 | |||
|} | |||
=Recipes on PECVD2 for deposition of silicon oxides <span style="color:Red">EXPIRED!!!</span>= | |||
==Quality control recipe (recipe changed in June 2015)== | |||
{| border="1" cellspacing="2" cellpadding="2" colspan="3" | |||
|bgcolor="#98FB98" |'''Quality Controle (QC) for PECVD2''' | |||
|- | |||
| | |||
{| {{table}} | |||
| align="center" | | |||
{| border="1" cellspacing="1" cellpadding="2" align="center" style="width:300px" | |||
! QC Recipe: | |||
! QCTOXIDE | |||
|- | |||
| SiH<sub>4</sub> flow | |||
|12 sccm | |||
|- | |||
|N<sub>2</sub>O flow | |||
|710 sccm | |||
|- | |||
|N<sub>2</sub> flow | |||
|392 sccm | |||
|- | |- | ||
| | |Pressure | ||
|~ | |700 mTorr | ||
|1. | |- | ||
|RF-power | |||
|150 W @380kHz | |||
|- | |||
|Deposition time | |||
|15 min | |||
|} | |||
| align="center" valign="top"| | |||
{| border="2" cellspacing="1" cellpadding="2" align="center" style="width:500px" | |||
!QC limits | |||
!PECVD2 | |||
|- | |||
|Deposition rate of Silicon Oxide | |||
|58 nm/min - 78nm/min | |||
|- | |||
|Non-uniformity of the deposition rate: ''(max-min)/2*AVG'' | |||
|<2% | |||
|- | |||
|Refractive index of the Silicon Oxide | |||
|1.45 - 1.48 | |||
|- | |||
|Non-uniformity of the refractive index: ''(max-min)/2*AVG'' | |||
|<0.2% | |||
|- | |||
|} | |||
|- | |||
|} | |||
|} | |||
==SiO2, High Rate <span style="color:Red">EXPIRED!!!</span>== | |||
{| border="1" style="text-align: center; width: 400px; height: 150px;" | |||
! colspan="2" style="text-align: center;" style="background: #efefef;" | 1SiO2HR | |||
|- | |||
!N<math>_2</math>O-flow | |||
|1600 sccm | |||
|- | |||
!SiH<math>_4</math>-flow | |||
|17 sccm | |||
|- | |||
!RF-power (380 kHz) | |||
|380 W | |||
|- | |||
!Process Pressure | |||
|400 mTorr | |||
|- | |||
!Deposition rate | |||
|179 nm/min (before 2014) | |||
|- | |||
!index of refraction | |||
|1.461 (before 2014) | |||
|} | |||
==SiO2 Low Rate <span style="color:Red">EXPIRED!!!</span>== | |||
{| border="1" style="text-align: center; width: 700px; height: 150px;" | |||
! colspan="2" style="text-align: left;" style="background: #efefef;" | 1OX_old | |||
! colspan="2" style="text-align: left;" style="background: #efefef;" | 1SiO2 (as QC) | |||
|- | |||
!N<math>_2</math>-flow | |||
|392 sccm | |||
|392 sccm | |||
|- | |||
!N<math>_2</math>O-flow | |||
|1420 sccm (setting in software is 710 sccm) | |||
|1420 sccm (setting in software is 710 sccm) | |||
|- | |||
!SiH<math>_4</math>-flow | |||
|12 sccm | |||
|12 sccm | |||
|- | |||
!RF-power | |||
|100 W | |||
|150 W | |||
|- | |||
!Process Pressure | |||
|550 mTorr | |||
|700 mTorr | |||
|- | |||
!Deposition rate | |||
|~100 nm/min | |||
| | |||
'''66 nm/min''' (2015-05-18 BGHE)<br> | |||
'''68-69 nm/min''' (2015-04-24 BGHE)<br> | |||
109 ± 2 nm/min [tested: 2014-03-18] ''Old shower head'' | |||
|- | |||
!index of refraction | |||
|1.47 | |||
| | |||
'''1.463-1.464''' (2015-04-24 BGHE)<br> | |||
1.465 [tested: 2014-03-18] ''Old shower head'' | |||
|- | |||
!Uniformity | |||
|<1 % | |||
| | |||
'''1%''' over the wafer (2015-04-24 BGHE)<br> | |||
3.2% over the wafer [tested: 2014-03-18] ''Old shower head'' | |||
|- | |||
!Comment | |||
|This recipe is not running stable. The load capacitor tunes to zero and that it cannot go further. The results in a small reflected power that is varying due to the bad matching. This lead to variations in results from time to time. You may use it if you like, but please expect some variation in deposition rate. | |||
|This recipe was developed because the old one didn't tune well. It may have a less good uniformity but should be more stable. | |||
|} | |||
===Deposition rate as a function of deposition time using 1Ox_old:=== | |||
{| border="1" style="text-align: center; width: 400px; height: 150px;" | |||
|- | |||
| | |||
Deposition time [s] | |||
|Oxide thickness [nm] | |||
|Expected naturally grown oxide [nm] | |||
|Deposition rate [nm/min] | |||
|- | |||
|15 | |||
|26.9 | |||
|2 | |||
|99.6 | |||
|- | |||
|30 | |||
|51.9 | |||
|2 | |||
|99.8 | |||
|- | |||
|60 | |||
|102.4 | |||
|2 | |||
|100.4 | |||
|- | |||
|60 | |||
|102.7 | |||
|2 | |||
|100.7 | |||
|- | |||
|120 | |||
|201.1 | |||
|2 | |2 | ||
|99.6 | |||
|} | |||
===Thickness uniformity of test wafer using the test recipe=== | |||
[[image:PECVD2 SiO2 Test20 wafer map.jpg|350x350px|left|thumb|Thickness uniformity of test wafer using the test recipe.]] | |||
<br clear="all" /> | |||
==BPSG: RI vs. B/P <span style="color:Red">EXPIRED!!!</span> == | |||
B2H6 flow and PH3 flow was varied to map the RI of different B2H6/PH3 ratios. <br> | |||
''Work done by BGHE@dtu in fall 2013'' <br> | |||
{| border="1" cellspacing="0" cellpadding="7" | |||
|- | |||
|Recipe name | |||
|SiH4 flow [sccm] | |||
|N<sub>2</sub>O flow [sccm] | |||
|N2 flow [sccm] | |||
|B2H6 flow [sccm] | |||
|PH3 flow [sccm] | |||
|Pressure [mTorr] | |||
|Power [W] | |||
|Description | |||
|- | |||
|1PBSG | |||
|17 | |||
|1600 | |||
|0 | |||
|See below | |||
|See below | |||
|500 | |||
|800LF | |||
|BPSG glass for waveguide cladding layer | |||
|} | |||
LF=Low Frequency | |||
{| border="1" style="text-align: center; width: 400px; height: 150px;" | |||
|- | |||
|Run number | |||
|PH3 flow | |||
|B2H6 flow | |||
|B2H6/PH3 | |||
|RI | |||
|Thickness | |||
|- | |||
|A1 | |||
|40 sccm | |||
|135 sccm | |||
|3.38 | |||
|1.4582 | |||
|3.28 µm | |||
|- | |||
|A2 | |||
|55 sccm | |||
|115 sccm | |||
|2.09 | |||
|1.4615 | |||
|3.13 µm | |||
|- | |||
|A3 | |||
|45 sccm | |||
|130 sccm | |||
|2.89 | |||
|1.4590 | |||
|3.13 µm | |||
|- | |||
|A4 | |||
|35 sccm | |||
|140 sccm | |||
|4.0 | |||
|1.4572 | |||
|3.22 µm | |||
|- | |||
|A5 | |||
|50 sccm | |||
|120 sccm | |||
|2.4 | |||
|1.4602 | |||
|3.14 µm | |||
|- | |- | ||
|} | |} | ||
[[File:PECVD2_RI_vs_B-P_graph.jpg]] | |||
<br clear="all" /> | |||
=Recipes on PECVD1 for deposition of silicon oxides <span style="color:Red">EXPIRED!!!</span>= | |||
===Recipes=== | ===Recipes=== | ||
{| border="1" cellspacing="0" cellpadding="7" | {| border="1" cellspacing="0" cellpadding="7" | ||
| Line 44: | Line 614: | ||
|Recipe name | |Recipe name | ||
|SiH4 flow [sccm] | |SiH4 flow [sccm] | ||
|N< | |N<sub>2</sub>O flow [sccm] | ||
|N2 flow [sccm] | |N2 flow [sccm] | ||
|B2H6 flow [sccm] | |||
|PH3 flow [sccm] | |||
|GeH4*100 flow [sccm] | |||
|Pressure [mTorr] | |Pressure [mTorr] | ||
|Power [W] | |Power [W] | ||
|Description | |Description | ||
|- | |- | ||
| | |1oxide/1ox_std/standard | ||
| | |17 | ||
| | |1600 | ||
| | |0 | ||
| | |0 | ||
|0 | |||
|0 | |||
|400 | |||
|380LF | |||
|Process control recipe. Developed for waveguides | |||
|- | |||
|1PBSG | |||
|17 | |||
|1600 | |||
|0 | |||
|135 | |||
|40 | |||
|0 | |||
|500 | |||
|800LF | |||
|Developed for waveguide top cladding by ''Haiyan Ou @DTU Photonics'. | |||
|- | |||
|BGE_PBSG | |||
|17 | |||
|1600 | |||
|0 | |||
|240 | |||
|60 | |60 | ||
| | |0 | ||
|500 | |||
|800LF | |||
|Low stress PBSG | |||
|- | |||
|HO_core | |||
|17 | |||
|1600 | |||
|300 | |||
|0 | |||
|0 | |||
|400 | |||
|400 | |||
|600LF | |||
|Developed by Haiyan Ou @fotonik@dtu | |||
|- | |||
|HO_top | |||
|17 | |||
|1600 | |||
|0 | |||
|107 | |||
|40 | |||
|0 | |||
|500 | |||
|800LF | |||
|Developed by Haiyan Ou @fotonik@dtu | |||
|- | |- | ||
|} | |} | ||
===Expected results=== | ===Expected results=== | ||
| Line 65: | Line 685: | ||
|- | |- | ||
|Recipe name | |Recipe name | ||
|Deposition rate [ | |Deposition rate [µm/min] | ||
|RI | |RI | ||
|Uniformity [%] | |Uniformity [%] | ||
|Comments | |||
|- | |- | ||
| | |1oxide/1ox_std/standard | ||
|~ | |~0.193 | ||
|~1. | |1.46 | ||
| | |2 | ||
|The latest measured values can be seen in the process control sheet in LabManager | |||
|- | |||
|1PBSG | |||
|~0.3 | |||
|1.458@633nm | |||
| | |||
| | |||
|- | |- | ||
|} | |} | ||
Latest revision as of 11:15, 21 January 2025
Feedback to this page: click here
The content on this page, including all images and pictures, was created by Berit Herstrøm @ DTU Nanolab (BGHE), unless otherwise stated.
At the moment DTU Nanolab has 2 PECVDs that can deposit silicon oxide with or without dopants of boron, phosphorus. PECVD1 and PECVD2 has been decommissioned and now we have PECVD3 and PECVD4. PECVD3 are for silicon based processing allowing wafers with small amount of metal (<5% wafer coverage). PECVD4 is for clean wafers both for silicon based materials and for III-V materials. Look at the PECVD page to learn more about the PECVDs at Nanolab. All though PECVD4 and PECVD3 are very much alike you cannot count on that a recipe on one system will give exactly the same results on the other system.
Deposition of SiO2 with PECVD4
| Quality Control (QC) for PECVD4 - oxide | ||||||||||||||||||||||
|
| Recipe | Dep. rate [nm/min] | RI | Unif. [%] | Stress [MPa] | Comments | SiH4 [sccm] | N2O [sccm] | N2 [sccm] | B2H6 | PH3 | Pressure [mTorr] | Power [W] | Load | Tune | Time [mm:ss] | Tested
|
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| LF SiO | 75-78 nm/min | 1.480-1.483 | ± 2.1-2.7% | compressive 309 MPa | Click for more results | 12 | 1420 | 392 | 550 mTorr | 60LF" | 1:15/13:00(stress) | February 2017 bghe | ||||
| HF SiO | 63-64 nm/min | 1.476-1.477 | ± 0.3-0.5% | Compressive: 250.5 MPa | Click for more results | 10 | 1420 | 392 | 900 mTorr | 30HF | 2:00/16:00(stress) | February 2017 bghe | ||||
| waveguide | 159.5 nm/min | 1.462 | ± 0.8% | Compressive: 121.9 MPa | 17 | 2000 | 300 mTorr | 700 LF | 40:00 | February 2017 bghe | ||||||
| BPSG | 259 nm/min | 1.4593 | ± 1.7% | Compressive: 36.7 MPa | Measured after anneal in Clad1000 | 17 | 1600 | 135 | 40 | 900 mTorr | 800 LF | 10:00/56:00(stress) | February 2017 bghe | |||
| BPSG low stress | 302 nm/min | 1.4598 | ± 1.7% | Compressive: 1.4 MPa | Measured after anneal in Clad1000 | 17 | 1600 | 240 | 60 | 500 mTorr | 800LF | 10:00 | February 2017 bghe |
Recipes on PECVD3 for deposition of silicon oxides
| Quality Control (QC) for PECVD3 - oxide | ||||||||||||||||||||||
|
Recipes
| Recipe name | SiH4 flow [sccm] | N2O flow [sccm] | N2 flow [sccm] | B2H6 flow [sccm] | PH3 flow [sccm] | Pressure [mTorr] | Power [W] | Description |
| LFSiO2 | 12 | 1420 | 392 | 0 | 0 | 700 | 150 | New QC implemented in April 2016 |
| LFSiO | 12 | 1420 | 392 | 0 | 0 | 550 | 60 | Uniform silicon oxide |
| 1PBSG | 17 | 1600 | 0 | 135 | 40 | 500 | 800 LF | BPSG glass for waveguide cladding layer |
LF=Low Frequency
Expected results
| Recipe name | Deposition rate [nm/min] | RI | Uniformity [%] | Stress | Comment |
| LFSiO2 | 105nm/min | 1.47 | ~1.5% | 400-402 MPa compressive stress by Anders Simonsen @nbi.ku.dk April 2016 | We have seen that this recipe does not deposit the first minute |
| LFSiO | ~75 | ~1.48 | <1 | not measured | . |
| 1PBSG | ~228 nm/min | . | ~17% | not measured | . |
Recipes on PECVD3 for deposition of doped oxide
Recipes
| Recipe name | SiH4 flow [sccm] | N2O flow [sccm] | N2 flow [sccm] | GeH4 flow [sccm] (scaled by 100) | B2H6 flow [sccm] | PH3 flow [sccm] | Pressure [mTorr] | Power [W] | Description |
| Core-Ge (not possible anymore as we have no Germanium) | 17 | 1600 | 300 | 300 | 0 | 0 | 400 | 600 LF | Process for germanium doped core layer developed by Haiyan Ou from DTU Photonics
Annnealing: Anneal bond furnace, recipe "core1100" |
| Top-BPSG | 17 | 1600 | 0 | 0 | 100 | 40 | 500 | 800 LF | Process for PBSG top clading layer developed by Haiyan Ou from DTU Photonics
Annnealing/oxidation: Anneal bond furnace, recipe "clad1000" |
Expected results
| Recipe name | Deposition rate [nm/min] | Refractive index |
| Core-Ge | ~188 nm/min | ~1.46969 |
| Top-BPSG | ~248 nm/min | ~1.458 |
Recipes on PECVD2 for deposition of silicon oxides EXPIRED!!!
Quality control recipe (recipe changed in June 2015)
| Quality Controle (QC) for PECVD2 | ||||||||||||||||||||||||||
|
SiO2, High Rate EXPIRED!!!
| 1SiO2HR | |
|---|---|
| NO-flow | 1600 sccm |
| SiH-flow | 17 sccm |
| RF-power (380 kHz) | 380 W |
| Process Pressure | 400 mTorr |
| Deposition rate | 179 nm/min (before 2014) |
| index of refraction | 1.461 (before 2014) |
SiO2 Low Rate EXPIRED!!!
| 1OX_old | 1SiO2 (as QC) | ||
|---|---|---|---|
| N-flow | 392 sccm | 392 sccm | |
| NO-flow | 1420 sccm (setting in software is 710 sccm) | 1420 sccm (setting in software is 710 sccm) | |
| SiH-flow | 12 sccm | 12 sccm | |
| RF-power | 100 W | 150 W | |
| Process Pressure | 550 mTorr | 700 mTorr | |
| Deposition rate | ~100 nm/min |
66 nm/min (2015-05-18 BGHE) | |
| index of refraction | 1.47 |
1.463-1.464 (2015-04-24 BGHE) | |
| Uniformity | <1 % |
1% over the wafer (2015-04-24 BGHE) | |
| Comment | This recipe is not running stable. The load capacitor tunes to zero and that it cannot go further. The results in a small reflected power that is varying due to the bad matching. This lead to variations in results from time to time. You may use it if you like, but please expect some variation in deposition rate. | This recipe was developed because the old one didn't tune well. It may have a less good uniformity but should be more stable. | |
Deposition rate as a function of deposition time using 1Ox_old:
|
Deposition time [s] |
Oxide thickness [nm] | Expected naturally grown oxide [nm] | Deposition rate [nm/min] |
| 15 | 26.9 | 2 | 99.6 |
| 30 | 51.9 | 2 | 99.8 |
| 60 | 102.4 | 2 | 100.4 |
| 60 | 102.7 | 2 | 100.7 |
| 120 | 201.1 | 2 | 99.6 |
Thickness uniformity of test wafer using the test recipe

BPSG: RI vs. B/P EXPIRED!!!
B2H6 flow and PH3 flow was varied to map the RI of different B2H6/PH3 ratios.
Work done by BGHE@dtu in fall 2013
| Recipe name | SiH4 flow [sccm] | N2O flow [sccm] | N2 flow [sccm] | B2H6 flow [sccm] | PH3 flow [sccm] | Pressure [mTorr] | Power [W] | Description |
| 1PBSG | 17 | 1600 | 0 | See below | See below | 500 | 800LF | BPSG glass for waveguide cladding layer |
LF=Low Frequency
| Run number | PH3 flow | B2H6 flow | B2H6/PH3 | RI | Thickness |
| A1 | 40 sccm | 135 sccm | 3.38 | 1.4582 | 3.28 µm |
| A2 | 55 sccm | 115 sccm | 2.09 | 1.4615 | 3.13 µm |
| A3 | 45 sccm | 130 sccm | 2.89 | 1.4590 | 3.13 µm |
| A4 | 35 sccm | 140 sccm | 4.0 | 1.4572 | 3.22 µm |
| A5 | 50 sccm | 120 sccm | 2.4 | 1.4602 | 3.14 µm |
Recipes on PECVD1 for deposition of silicon oxides EXPIRED!!!
Recipes
| Recipe name | SiH4 flow [sccm] | N2O flow [sccm] | N2 flow [sccm] | B2H6 flow [sccm] | PH3 flow [sccm] | GeH4*100 flow [sccm] | Pressure [mTorr] | Power [W] | Description |
| 1oxide/1ox_std/standard | 17 | 1600 | 0 | 0 | 0 | 0 | 400 | 380LF | Process control recipe. Developed for waveguides |
| 1PBSG | 17 | 1600 | 0 | 135 | 40 | 0 | 500 | 800LF | Developed for waveguide top cladding by Haiyan Ou @DTU Photonics'. |
| BGE_PBSG | 17 | 1600 | 0 | 240 | 60 | 0 | 500 | 800LF | Low stress PBSG |
| HO_core | 17 | 1600 | 300 | 0 | 0 | 400 | 400 | 600LF | Developed by Haiyan Ou @fotonik@dtu |
| HO_top | 17 | 1600 | 0 | 107 | 40 | 0 | 500 | 800LF | Developed by Haiyan Ou @fotonik@dtu |
Expected results
| Recipe name | Deposition rate [µm/min] | RI | Uniformity [%] | Comments |
| 1oxide/1ox_std/standard | ~0.193 | 1.46 | 2 | The latest measured values can be seen in the process control sheet in LabManager |
| 1PBSG | ~0.3 | 1.458@633nm |