'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Silicon_Oxide/Deposition_of_Silicon_Oxide_using_PECVD  click here]'''  
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Silicon_Oxide/Deposition_of_Silicon_Oxide_using_PECVD  click here]'''<br>
{{CC-bghe1}}




At the moment DANCHIP has 2(3) PECVDs that can deposite silicon oxide with or without dopants of Boron, Phosphorous or Germanium. PECVD1 has been decommissioned and PECVD3 are for silicon based processing allowing wafers with small abount of metal (<5% wafer coverage). PECVD2 is clean wafers both for silicon based materials and for III-V materials. At the moment PECVD2 is described under III-V processing. Look at the [[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]] page to learn more about the PECVDs at DANCHIP. All though PECVD2 and PECVD3 are very much alike you cannot count on the a recipe on one system will give exactly the same results on the other system.
At the moment DTU Nanolab has 2 PECVDs that can deposit silicon oxide with or without dopants of boron, phosphorus. PECVD1 and PECVD2 has been decommissioned and now we have PECVD3 and PECVD4. PECVD3 are for silicon based processing allowing wafers with small amount of metal (<5% wafer coverage). PECVD4 is for clean wafers both for silicon based materials and for III-V materials. Look at the [[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]] page to learn more about the PECVDs at Nanolab. All though PECVD4 and PECVD3 are very much alike you cannot count on that a recipe on one system will give exactly the same results on the other system.


=Recipes on PECVD2 for deposition of silicon oxides=
== Deposition of SiO2 with PECVD4 ==
See [[Specific Process Knowledge/III-V Process/thin film dep/pecvd2| here]]
 
==Quality control recipe==
{| border="1" cellspacing="2" cellpadding="2" colspan="3"
{| border="1" cellspacing="2" cellpadding="2" colspan="3"
|bgcolor="#98FB98" |'''Quality Controle (QC) for PECVD2'''
|bgcolor="#98FB98" |'''Quality Control (QC) for PECVD4 - oxide '''
|-
|-
|
|
*[http://labmanager.danchip.dtu.dk/d4Show.php?id=1988&mach=17 The QC procedure for PECVD2]<br>
*[http://labmanager.dtu.dk/d4Show.php?id=5093&mach=395 The QC procedure for PECVD4 - requires login]<br>
*[http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=17 The newest QC data for PECVD2]
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=395 The newest QC data for PECVD4 - requires login]
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |  
{| border="1" cellspacing="1" cellpadding="2"  align="center" style="width:300px"
{| border="1" cellspacing="1" cellpadding="2"  align="center" style="width:200px"


! QC Recipe:
! QC Recipe:
! QCTOXIDE
! QCOXYD2
|-  
|-  
| SiH<sub>4</sub> flow
| SiH<sub>4</sub> flow
Line 26: Line 23:
|-
|-
|N<sub>2</sub>O flow
|N<sub>2</sub>O flow
|710 sccm
|1420 sccm
|-
|-
|N<sub>2</sub> flow
|N<sub>2</sub> flow
|392 sccm
|392 sccm
|-  
|-  
|Pressure
|Pressure
Line 35: Line 33:
|-
|-
|RF-power
|RF-power
|100 W @380kHz
|60 W
|-
|-
|Deposition time
|1 min
|}
|}
| align="center" valign="top"|
| align="center" valign="top"|
{| border="2" cellspacing="1" cellpadding="2" align="center" style="width:500px"
{| border="2" cellspacing="1" cellpadding="2" align="center" style="width:500px"
!QC limits
!QC limits
!PECVD2
!PECVD4 - OXIDE
|-
|-
|Depostion rate of Silicon Oxide
|Deposition rate
|69nm/min - 119nm/min
|70 - 85 nm/min
|-
|-
|Non-uniformity of the deposition rate (std. deviation of 9 points)
|Non-uniformity
|0 - 2.8 nm
|<3.0
|-
|-
|Refractive index of the Silicon Oxide
|Refractive index
|1.41 - 1.53
|1.474 - 1.486
|-
|Non-uniformity of the refrative index (std. deviation of 9 points)
|0 - 0.07
|-
|-
|}
|}
Line 62: Line 55:
|}
|}


==SiO2 Standard, High Rate==
{| border="1" cellspacing="2" cellpadding="2"  
 
|-style="background:Black; color:White"
 
!|Recipe
 
!|Dep. rate [nm/min]
{| border="1" style="text-align: center; width: 400px; height: 150px;"
!|RI
! colspan="2" style="text-align: center;" style="background: #efefef;" | SiO2 Standard
!|Unif. [%]
|-
!|Stress [MPa]
!N<math>_2</math>O-flow
!|Comments
|1600 sccm
!|SiH4 [sccm]
!|N2O [sccm]
!|N2 [sccm]
!|B2H6
!|PH3
!|Pressure [mTorr]
!|Power [W]
!|Load
!|Tune
!|Time [mm:ss]
!|Tested
|-
|-
!SiH<math>_4</math>-flow
|LF SiO<!-- Recipe -->
|17 sccm
|75-78 nm/min<!-- Dep. rate [nm/min] -->
|1.480-1.483<!-- RI -->
|&plusmn; 2.1-2.7%<!-- Unif. [%] -->
|compressive 309 MPa <!-- Stress [MPa] -->
|[[/LF_SiO2 results|Click for more results]]<!-- Comments -->
|12<!-- SiH4 [sccm] -->
|1420<!-- N2O [sccm] -->
|392<!-- N2 [sccm] -->
|<!-- B2H6 -->
|<!-- PH3 -->
|550 mTorr<!-- Pressure [mTorr] -->
|60LF"<!-- Power [W] -->
|<!-- Load -->
|<!-- Tune -->
|1:15/13:00(stress)<!-- Time [mm:ss] -->
|February 2017 bghe<!--Tested -->
|-
|-
!RF-power (380 kHz)
|HF SiO<!-- Recipe -->
|380 W
|63-64 nm/min<!-- Dep. rate [nm/min] -->
|1.476-1.477<!-- RI -->
|&plusmn; 0.3-0.5%<!-- Unif. [%] -->
|Compressive: 250.5 MPa<!-- Stress [MPa] -->
|[[/HF_SiO2 results|Click for more results]]<!-- Comments -->
|10<!-- SiH4 [sccm] -->
|1420<!-- N2O [sccm] -->
|392<!-- N2 [sccm] -->
|<!-- B2H6 -->
|<!-- PH3 -->
|900 mTorr<!-- Pressure [mTorr] -->
|30HF<!-- Power [W] -->
|<!-- Load -->
|<!-- Tune -->
|2:00/16:00(stress)<!-- Time [mm:ss] -->
|February 2017 bghe<!--Tested -->
|-
|-
!Process Pressure
|waveguide <!-- Recipe -->
|400 mTorr
|159.5 nm/min<!-- Dep. rate [nm/min] -->
|1.462<!-- RI -->
|&plusmn; 0.8%<!-- Unif. [%] -->
|Compressive: 121.9 MPa<!-- Stress [MPa] -->
|<!-- Comments -->
|17<!-- SiH4 [sccm] -->
|2000<!-- N2O [sccm] -->
|<!-- N2 [sccm] -->
|<!-- B2H6 -->
|<!-- PH3 -->
|300 mTorr<!-- Pressure [mTorr] -->
|700 LF<!-- Power [W] -->
|<!-- Load -->
|<!-- Tune -->
|40:00<!-- Time [mm:ss] -->
|February 2017 bghe<!--Tested -->
|-
|-
!Deposition rate
|BPSG<!-- Recipe -->
|179 nm/min
|259 nm/min<!-- Dep. rate [nm/min] -->
|1.4593<!-- RI -->
|&plusmn; 1.7%<!-- Unif. [%] -->
|Compressive: 36.7 MPa<!-- Stress [MPa] -->
|Measured after anneal in Clad1000<!-- Comments -->
|17<!-- SiH4 [sccm] -->
|1600<!-- N2O [sccm] -->
|<!-- N2 [sccm] -->
|135<!-- B2H6 -->
|40<!-- PH3 -->
|900 mTorr<!-- Pressure [mTorr] -->
|800 LF <!-- Power [W] -->
|<!-- Load -->
|<!-- Tune -->
|10:00/56:00(stress)<!-- Time [mm:ss] -->
|February 2017 bghe <!--Tested -->
|-
|-
!index of refraction
|BPSG low stress<!-- Recipe -->
|1.461
|302 nm/min<!-- Dep. rate [nm/min] -->
|}
|1.4598<!-- RI -->
 
|&plusmn; 1.7%<!-- Unif. [%] -->
==SiO2 Standard, Low Rate==
|Compressive: 1.4 MPa<!-- Stress [MPa] -->
|Measured after anneal in Clad1000 <!-- Comments -->
|17<!-- SiH4 [sccm] -->
|1600<!-- N2O [sccm] -->
|<!-- N2 [sccm] -->
|240<!-- B2H6 -->
|60<!-- PH3 -->
|500 mTorr<!-- Pressure [mTorr] -->
|800LF<!-- Power [W] -->
|<!-- Load -->
|<!-- Tune -->
|10:00 <!-- Time [mm:ss] -->
|February 2017 bghe <!--Tested -->


{| border="1" style="text-align: center; width: 700px; height: 150px;"
! colspan="2" style="text-align: left;" style="background: #efefef;" | 1STOxide
! colspan="2" style="text-align: left;" style="background: #efefef;" | A test recipe
|-
|-
!N<math>_2</math>-flow
|392 sccm
|392 sccm
|-
!N<math>_2</math>O-flow
|1420 sccm (setting in software is 710 sccm)
|1420 sccm (setting in software is 710 sccm)
|-
!SiH<math>_4</math>-flow
|12 sccm
|12 sccm
|-
!RF-power
|100 W
|150 W
|-
!Process Pressure
|550 mTorr
|700 mTorr
|-
!Deposition rate
|~100 nm/min
|109 &plusmn; 2 nm/min [tested: 2014-03-18]
|-
!index of refraction
|1.47
|1.465 [tested: 2014-03-18]
|-
!Uniformity
|<1 %
|3.2% over the wafer [tested: 2014-03-18]
|}


===Deposition rate as a function of deposition time using 1STOxide:===
{| border="1" style="text-align: center; width: 400px; height: 150px;"
|-
|
Deposition time [s]
|Oxide thickness [nm]
|Expected naturally grown oxide [nm]
|Deposition rate [nm/min]
|-
|15
|26.9
|2
|99.6
|-
|30
|51.9
|2
|99.8
|-
|60
|102.4
|2
|100.4
|-
|60
|102.7
|2
|100.7
|-
|120
|201.1
|2
|99.6
|}
|}


 
*[[/conformity|SEM images of the conformity of the layer on a structured surface]]
===Thickness uniformity of test wafer using the test recipe===
[[image:PECVD2 SiO2 Test20 wafer map.jpg|350x350px|left|thumb|Thickness uniformity of test wafer using the test recipe.]]


<br clear="all" />
<br clear="all" />
==Silicon nitride==
{| border="1" cellspacing="0" cellpadding="7"
|-
|Recipe name
|SiH4 flow [sccm]
|NH3 flow [sccm]
|N2 flow [sccm]
|Pressure [mTorr]
|Power [W]
|Description
|-
|1nitride
|30
|20
|1000
|500
|80
|
|-
|}


=Recipes on PECVD3 for deposition of silicon oxides=
=Recipes on PECVD3 for deposition of silicon oxides=
{| border="1" cellspacing="2" cellpadding="2" colspan="3"
{| border="1" cellspacing="2" cellpadding="2" colspan="3"
|bgcolor="#98FB98" |'''Quality Controle (QC) for PECVD3 - oxide'''
|bgcolor="#98FB98" |'''Quality Control (QC) for PECVD3 - oxide'''
|-
|-
|
|
*[http://labmanager.danchip.dtu.dk/d4Show.php?id=1402&mach=106 The QC procedure for PECVD3]<br>
*[http://labmanager.dtu.dk/d4Show.php?id=1402&mach=106 The QC procedure for PECVD3 - requires login]<br>
*[http://www.labmanager.danchip.dtu.dk/view_binary.php?type=data&mach=106 The newest QC data for PECVD3]
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=106 The newest QC data for PECVD3 - requires login]
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |  
Line 204: Line 187:


! QC Recipe:
! QC Recipe:
! QCOXYD
! QCOXYD2
|-  
|-  
| SiH<sub>4</sub> flow
| SiH<sub>4</sub> flow
Line 217: Line 200:
|-  
|-  
|Pressure
|Pressure
|550 mTorr
|700 mTorr
|-
|-
|RF-power
|RF-power
|60 W
|150 W
|-
|-
|}
|}
Line 229: Line 212:
|-
|-
|Deposition rate
|Deposition rate
|66 - 89 nm/min
|97 - 112 nm/min
|-
|-
|Non-uniformity
|Non-uniformity
|<1.9%
|<2.0
|-
|-
|Refractive index
|Refractive index
|1.472 - 1.487
|1.467 - 1.474
|-
|-
|}
|}
Line 254: Line 237:
|Power [W]
|Power [W]
|Description
|Description
|-
|LFSiO2
|12
|1420
|392
|0
|0
|700
|150
|New QC implemented in April 2016
|-  
|-  
|LFSiO
|LFSiO
Line 272: Line 265:
|40
|40
|500
|500
|800LF
|800 LF
|BPSG glass for waveguide cladding layer  
|BPSG glass for waveguide cladding layer  
|}
|}
Line 284: Line 277:
|RI
|RI
|Uniformity [%]
|Uniformity [%]
|Stress
|Comment
|-
|LFSiO2
|105nm/min
|1.47
|~1.5%
|'''400-402 MPa''' compressive stress '' by Anders Simonsen @nbi.ku.dk April 2016''
|We have seen that this recipe does not deposit the first minute
|-  
|-  
|LFSiO
|LFSiO
Line 289: Line 291:
|~1.48
|~1.48
|<1
|<1
|not measured
|.
|-
|-
|1PBSG
|1PBSG
Line 294: Line 298:
|.
|.
|~17%
|~17%
|not measured
|.
|}
|}
<br clear="all" />


=Recipes on PECVD3 for deposition of doped oxide=
=Recipes on PECVD3 for deposition of doped oxide=
Line 311: Line 318:
|Description
|Description
|-  
|-  
|Core-Ge
|Core-Ge (not possible anymore as we have no Germanium)
|17
|17
|1600
|1600
Line 352: Line 359:
|}
|}


=Recipes on PECVD2 for deposition of silicon oxides <span style="color:Red">EXPIRED!!!</span>=
==Quality control recipe (recipe changed in June 2015)==
{| border="1" cellspacing="2" cellpadding="2" colspan="3"
|bgcolor="#98FB98" |'''Quality Controle (QC) for PECVD2'''
|-
|
{| {{table}}
| align="center" |
{| border="1" cellspacing="1" cellpadding="2"  align="center" style="width:300px"
! QC Recipe:
! QCTOXIDE
|-
| SiH<sub>4</sub> flow
|12 sccm
|-
|N<sub>2</sub>O flow
|710 sccm
|-
|N<sub>2</sub> flow
|392 sccm
|-
|Pressure
|700 mTorr
|-
|RF-power
|150 W @380kHz
|-
|Deposition time
|15 min
|}
| align="center" valign="top"|
{| border="2" cellspacing="1" cellpadding="2" align="center" style="width:500px"
!QC limits
!PECVD2
|-
|Deposition rate of Silicon Oxide
|58 nm/min - 78nm/min
|-
|Non-uniformity of the deposition rate: ''(max-min)/2*AVG''
|<2%
|-
|Refractive index of the Silicon Oxide
|1.45 - 1.48
|-
|Non-uniformity of the refractive index: ''(max-min)/2*AVG''
|<0.2%
|-
|}
|-
|}
|}
==SiO2, High Rate <span style="color:Red">EXPIRED!!!</span>==
{| border="1" style="text-align: center; width: 400px; height: 150px;"
! colspan="2" style="text-align: center;" style="background: #efefef;" | 1SiO2HR
|-
!N<math>_2</math>O-flow
|1600 sccm
|-
!SiH<math>_4</math>-flow
|17 sccm
|-
!RF-power (380 kHz)
|380 W
|-
!Process Pressure
|400 mTorr
|-
!Deposition rate
|179 nm/min (before 2014)
|-
!index of refraction
|1.461 (before 2014)
|}
==SiO2 Low Rate <span style="color:Red">EXPIRED!!!</span>==
{| border="1" style="text-align: center; width: 700px; height: 150px;"
! colspan="2" style="text-align: left;" style="background: #efefef;" | 1OX_old
! colspan="2" style="text-align: left;" style="background: #efefef;" | 1SiO2 (as QC)
|-
!N<math>_2</math>-flow
|392 sccm
|392 sccm
|-
!N<math>_2</math>O-flow
|1420 sccm (setting in software is 710 sccm)
|1420 sccm (setting in software is 710 sccm)
|-
!SiH<math>_4</math>-flow
|12 sccm
|12 sccm
|-
!RF-power
|100 W
|150 W
|-
!Process Pressure
|550 mTorr
|700 mTorr
|-
!Deposition rate
|~100 nm/min
|
'''66 nm/min''' (2015-05-18 BGHE)<br>
'''68-69 nm/min''' (2015-04-24 BGHE)<br>
109 &plusmn; 2 nm/min [tested: 2014-03-18] ''Old shower head''
|-
!index of refraction
|1.47
|
'''1.463-1.464''' (2015-04-24 BGHE)<br>
1.465 [tested: 2014-03-18] ''Old shower head''
|-
!Uniformity
|<1 %
|
'''1%''' over the wafer (2015-04-24 BGHE)<br>
3.2% over the wafer [tested: 2014-03-18] ''Old shower head''
|-
!Comment
|This recipe is not running stable. The load capacitor tunes to zero and that it cannot go further. The results in a small reflected power that is varying due to the bad matching. This lead to variations in results from time to time. You may use it if you like, but please expect some variation in deposition rate.
|This recipe was developed because the old one didn't tune well. It may have a less good uniformity but should be more stable.
|}
===Deposition rate as a function of deposition time using 1Ox_old:===
{| border="1" style="text-align: center; width: 400px; height: 150px;"
|-
|
Deposition time [s]
|Oxide thickness [nm]
|Expected naturally grown oxide [nm]
|Deposition rate [nm/min]
|-
|15
|26.9
|2
|99.6
|-
|30
|51.9
|2
|99.8
|-
|60
|102.4
|2
|100.4
|-
|60
|102.7
|2
|100.7
|-
|120
|201.1
|2
|99.6
|}
===Thickness uniformity of test wafer using the test recipe===
[[image:PECVD2 SiO2 Test20 wafer map.jpg|350x350px|left|thumb|Thickness uniformity of test wafer using the test recipe.]]
<br clear="all" />
==BPSG: RI vs. B/P <span style="color:Red">EXPIRED!!!</span> ==
B2H6 flow and PH3 flow was varied to map the RI of different B2H6/PH3 ratios. <br>
''Work done by BGHE@dtu in fall 2013'' <br>
{| border="1" cellspacing="0" cellpadding="7"
|-
|Recipe name
|SiH4 flow [sccm]
|N<sub>2</sub>O flow [sccm]
|N2 flow [sccm]
|B2H6 flow [sccm]
|PH3 flow [sccm]
|Pressure [mTorr]
|Power [W]
|Description
|-
|1PBSG
|17
|1600
|0
|See below
|See below
|500
|800LF
|BPSG glass for waveguide cladding layer
|}
LF=Low Frequency
{| border="1" style="text-align: center; width: 400px; height: 150px;"
|-
|Run number
|PH3 flow
|B2H6 flow
|B2H6/PH3
|RI
|Thickness
|-
|A1
|40 sccm
|135 sccm
|3.38
|1.4582
|3.28 µm
|-
|A2
|55 sccm
|115 sccm
|2.09
|1.4615
|3.13 µm
|-
|A3
|45 sccm
|130 sccm
|2.89
|1.4590
|3.13 µm
|-
|A4
|35 sccm
|140 sccm
|4.0
|1.4572
|3.22 µm
|-
|A5
|50 sccm
|120 sccm
|2.4
|1.4602
|3.14 µm
|-
|}
[[File:PECVD2_RI_vs_B-P_graph.jpg]]
<br clear="all" />


=Recipes on PECVD1 for deposition of silicon oxides <span style="color:Red">Expired!</span>=
=Recipes on PECVD1 for deposition of silicon oxides <span style="color:Red">EXPIRED!!!</span>=
===Recipes===
===Recipes===
{| border="1" cellspacing="0" cellpadding="7"
{| border="1" cellspacing="0" cellpadding="7"

Latest revision as of 11:15, 21 January 2025

Feedback to this page: click here
The content on this page, including all images and pictures, was created by Berit Herstrøm @ DTU Nanolab (BGHE), unless otherwise stated.


At the moment DTU Nanolab has 2 PECVDs that can deposit silicon oxide with or without dopants of boron, phosphorus. PECVD1 and PECVD2 has been decommissioned and now we have PECVD3 and PECVD4. PECVD3 are for silicon based processing allowing wafers with small amount of metal (<5% wafer coverage). PECVD4 is for clean wafers both for silicon based materials and for III-V materials. Look at the PECVD page to learn more about the PECVDs at Nanolab. All though PECVD4 and PECVD3 are very much alike you cannot count on that a recipe on one system will give exactly the same results on the other system.

Deposition of SiO2 with PECVD4

Quality Control (QC) for PECVD4 - oxide
QC Recipe: QCOXYD2
SiH4 flow 12 sccm
N2O flow 1420 sccm
N2 flow 392 sccm
Pressure 550 mTorr
RF-power 60 W
QC limits PECVD4 - OXIDE
Deposition rate 70 - 85 nm/min
Non-uniformity <3.0
Refractive index 1.474 - 1.486
Recipe Dep. rate [nm/min] RI Unif. [%] Stress [MPa] Comments SiH4 [sccm] N2O [sccm] N2 [sccm] B2H6 PH3 Pressure [mTorr] Power [W] Load Tune Time [mm:ss] Tested


LF SiO 75-78 nm/min 1.480-1.483 ± 2.1-2.7% compressive 309 MPa Click for more results 12 1420 392 550 mTorr 60LF" 1:15/13:00(stress) February 2017 bghe
HF SiO 63-64 nm/min 1.476-1.477 ± 0.3-0.5% Compressive: 250.5 MPa Click for more results 10 1420 392 900 mTorr 30HF 2:00/16:00(stress) February 2017 bghe
waveguide 159.5 nm/min 1.462 ± 0.8% Compressive: 121.9 MPa 17 2000 300 mTorr 700 LF 40:00 February 2017 bghe
BPSG 259 nm/min 1.4593 ± 1.7% Compressive: 36.7 MPa Measured after anneal in Clad1000 17 1600 135 40 900 mTorr 800 LF 10:00/56:00(stress) February 2017 bghe
BPSG low stress 302 nm/min 1.4598 ± 1.7% Compressive: 1.4 MPa Measured after anneal in Clad1000 17 1600 240 60 500 mTorr 800LF 10:00 February 2017 bghe


Recipes on PECVD3 for deposition of silicon oxides

Quality Control (QC) for PECVD3 - oxide
QC Recipe: QCOXYD2
SiH4 flow 12 sccm
N2O flow 1420 sccm
N2 flow 392 sccm
Pressure 700 mTorr
RF-power 150 W
QC limits PECVD3 - OXIDE
Deposition rate 97 - 112 nm/min
Non-uniformity <2.0
Refractive index 1.467 - 1.474

Recipes

Recipe name SiH4 flow [sccm] N2O flow [sccm] N2 flow [sccm] B2H6 flow [sccm] PH3 flow [sccm] Pressure [mTorr] Power [W] Description
LFSiO2 12 1420 392 0 0 700 150 New QC implemented in April 2016
LFSiO 12 1420 392 0 0 550 60 Uniform silicon oxide
1PBSG 17 1600 0 135 40 500 800 LF BPSG glass for waveguide cladding layer

LF=Low Frequency

Expected results

Recipe name Deposition rate [nm/min] RI Uniformity [%] Stress Comment
LFSiO2 105nm/min 1.47 ~1.5% 400-402 MPa compressive stress by Anders Simonsen @nbi.ku.dk April 2016 We have seen that this recipe does not deposit the first minute
LFSiO ~75 ~1.48 <1 not measured .
1PBSG ~228 nm/min . ~17% not measured .


Recipes on PECVD3 for deposition of doped oxide

Recipes

Recipe name SiH4 flow [sccm] N2O flow [sccm] N2 flow [sccm] GeH4 flow [sccm] (scaled by 100) B2H6 flow [sccm] PH3 flow [sccm] Pressure [mTorr] Power [W] Description
Core-Ge (not possible anymore as we have no Germanium) 17 1600 300 300 0 0 400 600 LF Process for germanium doped core layer developed by Haiyan Ou from DTU Photonics

Annnealing: Anneal bond furnace, recipe "core1100"

Top-BPSG 17 1600 0 0 100 40 500 800 LF Process for PBSG top clading layer developed by Haiyan Ou from DTU Photonics

Annnealing/oxidation: Anneal bond furnace, recipe "clad1000"

Expected results

Recipe name Deposition rate [nm/min] Refractive index
Core-Ge ~188 nm/min ~1.46969
Top-BPSG ~248 nm/min ~1.458

Recipes on PECVD2 for deposition of silicon oxides EXPIRED!!!

Quality control recipe (recipe changed in June 2015)

Quality Controle (QC) for PECVD2
QC Recipe: QCTOXIDE
SiH4 flow 12 sccm
N2O flow 710 sccm
N2 flow 392 sccm
Pressure 700 mTorr
RF-power 150 W @380kHz
Deposition time 15 min
QC limits PECVD2
Deposition rate of Silicon Oxide 58 nm/min - 78nm/min
Non-uniformity of the deposition rate: (max-min)/2*AVG <2%
Refractive index of the Silicon Oxide 1.45 - 1.48
Non-uniformity of the refractive index: (max-min)/2*AVG <0.2%

SiO2, High Rate EXPIRED!!!

1SiO2HR
N2O-flow 1600 sccm
SiH4-flow 17 sccm
RF-power (380 kHz) 380 W
Process Pressure 400 mTorr
Deposition rate 179 nm/min (before 2014)
index of refraction 1.461 (before 2014)

SiO2 Low Rate EXPIRED!!!

1OX_old 1SiO2 (as QC)
N2-flow 392 sccm 392 sccm
N2O-flow 1420 sccm (setting in software is 710 sccm) 1420 sccm (setting in software is 710 sccm)
SiH4-flow 12 sccm 12 sccm
RF-power 100 W 150 W
Process Pressure 550 mTorr 700 mTorr
Deposition rate ~100 nm/min

66 nm/min (2015-05-18 BGHE)
68-69 nm/min (2015-04-24 BGHE)
109 ± 2 nm/min [tested: 2014-03-18] Old shower head

index of refraction 1.47

1.463-1.464 (2015-04-24 BGHE)
1.465 [tested: 2014-03-18] Old shower head

Uniformity <1 %

1% over the wafer (2015-04-24 BGHE)
3.2% over the wafer [tested: 2014-03-18] Old shower head

Comment This recipe is not running stable. The load capacitor tunes to zero and that it cannot go further. The results in a small reflected power that is varying due to the bad matching. This lead to variations in results from time to time. You may use it if you like, but please expect some variation in deposition rate. This recipe was developed because the old one didn't tune well. It may have a less good uniformity but should be more stable.


Deposition rate as a function of deposition time using 1Ox_old:

Deposition time [s]

Oxide thickness [nm] Expected naturally grown oxide [nm] Deposition rate [nm/min]
15 26.9 2 99.6
30 51.9 2 99.8
60 102.4 2 100.4
60 102.7 2 100.7
120 201.1 2 99.6

Thickness uniformity of test wafer using the test recipe

Thickness uniformity of test wafer using the test recipe.


BPSG: RI vs. B/P EXPIRED!!!

B2H6 flow and PH3 flow was varied to map the RI of different B2H6/PH3 ratios.
Work done by BGHE@dtu in fall 2013

Recipe name SiH4 flow [sccm] N2O flow [sccm] N2 flow [sccm] B2H6 flow [sccm] PH3 flow [sccm] Pressure [mTorr] Power [W] Description
1PBSG 17 1600 0 See below See below 500 800LF BPSG glass for waveguide cladding layer

LF=Low Frequency

Run number PH3 flow B2H6 flow B2H6/PH3 RI Thickness
A1 40 sccm 135 sccm 3.38 1.4582 3.28 µm
A2 55 sccm 115 sccm 2.09 1.4615 3.13 µm
A3 45 sccm 130 sccm 2.89 1.4590 3.13 µm
A4 35 sccm 140 sccm 4.0 1.4572 3.22 µm
A5 50 sccm 120 sccm 2.4 1.4602 3.14 µm


Recipes on PECVD1 for deposition of silicon oxides EXPIRED!!!

Recipes

Recipe name SiH4 flow [sccm] N2O flow [sccm] N2 flow [sccm] B2H6 flow [sccm] PH3 flow [sccm] GeH4*100 flow [sccm] Pressure [mTorr] Power [W] Description
1oxide/1ox_std/standard 17 1600 0 0 0 0 400 380LF Process control recipe. Developed for waveguides
1PBSG 17 1600 0 135 40 0 500 800LF Developed for waveguide top cladding by Haiyan Ou @DTU Photonics'.
BGE_PBSG 17 1600 0 240 60 0 500 800LF Low stress PBSG
HO_core 17 1600 300 0 0 400 400 600LF Developed by Haiyan Ou @fotonik@dtu
HO_top 17 1600 0 107 40 0 500 800LF Developed by Haiyan Ou @fotonik@dtu

Expected results

Recipe name Deposition rate [µm/min] RI Uniformity [%] Comments
1oxide/1ox_std/standard ~0.193 1.46 2 The latest measured values can be seen in the process control sheet in LabManager
1PBSG ~0.3 1.458@633nm