Specific Process Knowledge/Lithography/UVLithography: Difference between revisions
No edit summary |
|||
(7 intermediate revisions by the same user not shown) | |||
Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php | {{cc-nanolab}} | ||
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Lithography/UVLithography click here]''' | |||
[[Category: Equipment|Lithography]] | |||
[[Category: Lithography]] | |||
[[Image:UVLithography.jpg|320x320px|right|]] | [[Image:UVLithography.jpg|320x320px|right|]] | ||
__TOC__ | |||
UV Lithography uses ultraviolet light to transfer a pattern from a photo-mask or a design file to a wafer coated with photoresist. The photoresist film is spin coated onto the wafers, the design is transferred to the resist by using an aligner, and subsequently the resist pattern is developed. DTU Nanolab houses a number of automatic or manual coaters, mask or maskless aligners, as well as automatic or semi-automatic developers. | UV Lithography uses ultraviolet light to transfer a pattern from a photo-mask or a design file to a wafer coated with photoresist. The photoresist film is spin coated onto the wafers, the design is transferred to the resist by using an aligner, and subsequently the resist pattern is developed. DTU Nanolab houses a number of automatic or manual coaters, mask or maskless aligners, as well as automatic or semi-automatic developers. | ||
Line 20: | Line 27: | ||
'''Pre-cleanroom work:''' | '''Pre-cleanroom work:''' | ||
#'''Complete the TPT Lithography course''': [[LabAdviser/Courses/TPT_Lithography|Lithography Tool Package Training]]. | #'''Complete the TPT Lithography course''': [[LabAdviser/Courses/TPT_Lithography|Lithography Tool Package Training]]. | ||
#'''Prepare a process flow''' | #'''Prepare a process flow:''' The process flow describes all steps in your UV lithography process. You can find docx-templates <u>[[Specific_Process_Knowledge/Lithography/Resist/UVresist#UV_resist_comparison_table|in this table]]</u>. | ||
#'''Design device''': Design your device and layout. A detailed instruction on how to design a layout (mask) can be found <u>[[Specific_Process_Knowledge/Pattern_Design|here]]</u>. | #'''Design device''': Design your device and layout. A detailed instruction on how to design a layout (or mask) can be found <u>[[Specific_Process_Knowledge/Pattern_Design|here]]</u>. | ||
#'''Mask''': If you wish to use a mask aligner, order a photomask for your UV process. Instructions on how to order a photomask can be found <u>[[Specific_Process_Knowledge/Pattern_Design#Mask_Ordering_and_Fabrication|here]]</u>. | #'''Mask''': If you wish to use a mask aligner, order a photomask for your UV process. Instructions on how to order a photomask can be found <u>[[Specific_Process_Knowledge/Pattern_Design#Mask_Ordering_and_Fabrication|here]]</u>. | ||
'''Cleanroom work:''' | '''Cleanroom work:''' | ||
#'''Substrate pretreatment''': In many processes it is recommended to <u>[[Specific_Process_Knowledge/Lithography/Pretreatment|pretreat or prime]]</u> your wafer before spin-coating. In some <u>[[Specific_Process_Knowledge/Lithography/Coaters|spin-coaters]]</u>, these pretreatment processes are included in the spin coating of resist. | #'''Substrate pretreatment''': In many processes it is recommended to <u>[[Specific_Process_Knowledge/Lithography/Pretreatment|pretreat or prime]]</u> your wafer before spin-coating. In some <u>[[Specific_Process_Knowledge/Lithography/Coaters|spin-coaters]]</u>, these pretreatment processes are included in the spin coating of resist. | ||
#'''Resist Type''': Choose the type of resist you wish to use: a list of UV lithography resist types available at DTU Nanolab can be found <u>[[Specific_Process_Knowledge/Lithography/Resist | #'''Resist Type''': Choose the type of resist you wish to use: a list of UV lithography resist types available at DTU Nanolab can be found <u>[[Specific_Process_Knowledge/Lithography/Resist#UV_Resist|on this page]]</u>. | ||
# | #*Positive tone resist: Resist exposed to UV light will be dissolved in the developer. For mask aligners, the mask openings are an exact copy of the resist pattern which is to remain on the wafer. | ||
# | #*Negative tone resist: Resist exposed to UV light will become polymerized and difficult to dissolve. For mask aligners, the mask openings are an ''inverse'' copy of the resist pattern which is to remain on the wafer. | ||
#'''Thickness of resist''': In general, it is recommended to work at or below an aspect ratio of ~1, i.e. where the | #'''Thickness of resist''': In general, it is recommended to work at, or below, an aspect ratio of ~1, i.e. where the feature sizes of the pattern, is larger than the thickness of the resist. Furthermore, when you decide on the resist thickness, consider which transfer you need: | ||
# | #*For <u>[[Specific_Process_Knowledge/Lithography/LiftOff|lift-off]]</u> processes, we recommend resist thickness at least 5 times larger than the thickness of the metal to be lifted. | ||
# | #*For dry etch or wet etch processes, investigate the resist etch rate of your process, as this might limit the ''minimum'' thickness of your resist. | ||
#'''Spin Coater''': Do you wish to use a manual spin coater or an automatic spin coater? See a list of spin coaters <u>[[Specific_Process_Knowledge/Lithography/Coaters|here]]</u>. | #'''Spin Coater''': Do you wish to use a manual spin coater or an automatic spin coater? See a list of spin coaters <u>[[Specific_Process_Knowledge/Lithography/Coaters|here]]</u>. | ||
#'''Exposure''': Choose which aligner you wish to use, and consider the exposure dose. | #'''Exposure''': Choose which aligner you wish to use, and consider the exposure dose. | ||
# | #*You can find a list of mask aligners and maskless aligners <u>[[Specific_Process_Knowledge/Lithography/UVExposure|here]]</u>. | ||
# | #*You can find information on dose <u>[[Specific_Process_Knowledge/Lithography/Resist#UV_Resist|here]]</u>. | ||
#'''Development''': Choose which equipment you wish to use to develop your photoresist from <u>[[Specific_Process_Knowledge/Lithography/Development|this list]]</u>. Remember the development process influences the <u>[[Specific_Process_Knowledge/Lithography/Resist | #'''Development''': Choose which equipment you wish to use to develop your photoresist from <u>[[Specific_Process_Knowledge/Lithography/Development|this list]]</u>. Remember the development process influences the <u>[[Specific_Process_Knowledge/Lithography/Resist#UV_Resist|exposure dose]]</u>. | ||
#'''Specify whether you wish to strip or lift-off your resist''': <u>[[Specific_Process_Knowledge/Lithography/Strip|strip]]</u> and <u>[[Specific_Process_Knowledge/Lithography/LiftOff|lift-off]]</u>. | #'''Specify whether you wish to strip or lift-off your resist''': <u>[[Specific_Process_Knowledge/Lithography/Strip|strip]]</u> and <u>[[Specific_Process_Knowledge/Lithography/LiftOff|lift-off]]</u>. | ||
Line 43: | Line 50: | ||
=Process information= | =Process information= | ||
===[[Specific Process Knowledge/Lithography/Resist | ===[[Specific Process Knowledge/Lithography/Resist#UV_Resist|UV Resist]]=== | ||
===[[Specific Process Knowledge/Lithography/Pretreatment|Pretreatment]]=== | ===[[Specific Process Knowledge/Lithography/Pretreatment|Pretreatment]]=== | ||
===[[Specific Process Knowledge/Lithography/Coaters|Coating]]=== | ===[[Specific Process Knowledge/Lithography/Coaters|Coating]]=== | ||
===[[Specific Process Knowledge/Lithography/Baking|Baking]]=== | ===[[Specific Process Knowledge/Lithography/Baking|Baking]]=== | ||
===[[Specific Process Knowledge/Lithography/UVExposure|UV Exposure]]=== | ===[[Specific Process Knowledge/Lithography/UVExposure|UV Exposure Tools]]=== | ||
===[[Specific Process Knowledge/Lithography/Development|Development]]=== | ===[[Specific Process Knowledge/Lithography/Development|Development]]=== | ||
===[[Specific Process Knowledge/Lithography/Descum|Descum]]=== | ===[[Specific Process Knowledge/Lithography/Descum|Descum]]=== |
Latest revision as of 14:44, 10 May 2023
The contents on this page, including all images and pictures, was created by DTU Nanolab staff unless otherwise stated.
Feedback to this page: click here
UV Lithography uses ultraviolet light to transfer a pattern from a photo-mask or a design file to a wafer coated with photoresist. The photoresist film is spin coated onto the wafers, the design is transferred to the resist by using an aligner, and subsequently the resist pattern is developed. DTU Nanolab houses a number of automatic or manual coaters, mask or maskless aligners, as well as automatic or semi-automatic developers.
Getting started
Before you plan your UV processing and request for training on any equipment in UV lithography, please go through the following steps. Include the information in the training request.
Also, please remember that the Lithography Tool Package Training is mandatory before training in any lithography equipment.
If you are new to photolithography, you can visit this wikipedia webpage about photolithography before you start.
Pre-cleanroom work:
- Complete the TPT Lithography course: Lithography Tool Package Training.
- Prepare a process flow: The process flow describes all steps in your UV lithography process. You can find docx-templates in this table.
- Design device: Design your device and layout. A detailed instruction on how to design a layout (or mask) can be found here.
- Mask: If you wish to use a mask aligner, order a photomask for your UV process. Instructions on how to order a photomask can be found here.
Cleanroom work:
- Substrate pretreatment: In many processes it is recommended to pretreat or prime your wafer before spin-coating. In some spin-coaters, these pretreatment processes are included in the spin coating of resist.
- Resist Type: Choose the type of resist you wish to use: a list of UV lithography resist types available at DTU Nanolab can be found on this page.
- Positive tone resist: Resist exposed to UV light will be dissolved in the developer. For mask aligners, the mask openings are an exact copy of the resist pattern which is to remain on the wafer.
- Negative tone resist: Resist exposed to UV light will become polymerized and difficult to dissolve. For mask aligners, the mask openings are an inverse copy of the resist pattern which is to remain on the wafer.
- Thickness of resist: In general, it is recommended to work at, or below, an aspect ratio of ~1, i.e. where the feature sizes of the pattern, is larger than the thickness of the resist. Furthermore, when you decide on the resist thickness, consider which transfer you need:
- For lift-off processes, we recommend resist thickness at least 5 times larger than the thickness of the metal to be lifted.
- For dry etch or wet etch processes, investigate the resist etch rate of your process, as this might limit the minimum thickness of your resist.
- Spin Coater: Do you wish to use a manual spin coater or an automatic spin coater? See a list of spin coaters here.
- Exposure: Choose which aligner you wish to use, and consider the exposure dose.
- Development: Choose which equipment you wish to use to develop your photoresist from this list. Remember the development process influences the exposure dose.
- Specify whether you wish to strip or lift-off your resist: strip and lift-off.
Process information
UV Resist
Pretreatment
Coating
Baking
UV Exposure Tools
Development
Descum
Lift-off
Stripping Resist
Information from our suppliers
Application notes from MicroChemicals GmbH, e.g. Lithography Trouble-Shooter