{{:Specific Process Knowledge/Lithography/Strip/plasmaAsher03}}
Typical process time for stripping in plasma asher 1 or 2:
{{:Specific Process Knowledge/Lithography/Strip/plasmaAsher04}}
*1.5 µm AZ 5214E resist film: ~15 min
*10 µm AZ 4562 resist film: ~45 min
Typical process parameters:
{{:Specific Process Knowledge/Lithography/Strip/plasmaAsher05}}
*O<sub>2</sub>: 400 ml/min
*N<sub>2</sub>: 70 ml/min
*Power: 1000 W
{{:Specific Process Knowledge/Lithography/Strip/resistStrip}}
A typical descum process in plasma asher 1 or 2:
{{:Specific Process Knowledge/Lithography/Strip/wetBench06and07}}
*O<sub>2</sub>: 70 ml/min
*N<sub>2</sub>: 70 ml/min
*Power: 150 W
*Time : 10 min
=Decommisioned tools=
Be sure to wait for chamber to cool down to room temperature, before runinng descum processes in plasma asher 1 or 2. At a load of 2 Fused silica wafers, the amount of resist removed will be 10 - 1500 nm.
'''NB: Use dedicated descum asher Plasma Asher 3: Descum for descumming.'''
==Plasma Asher 1==
<span style="color:red">Plasma asher 1 was decommissioned 2024-12-02.</span>
<span style="color:red">Plasma asher 1 was decommissioned 2024-12-02.</span>
===[[Specific Process Knowledge/Lithography/Strip/PlasmaAsher1|Information about decommissioned tool]]===
[[Specific Process Knowledge/Lithography/Strip/PlasmaAsher1|Information about decommissioned tool can be found here.]]
==Plasma Asher 2==
[[Image:Plasma_Asher_6inch.jpg|300x300px|thumb|Plasma asher for removing AZ resist on 6" wafers: positioned in E-5]]
The Plasma Asher 2 is the same as Plasma Asher 1 but has another loading system which is more convenient for batch loading of 6inch substrates.
<span style="color:red">Plasma asher 2 was decommissioned 2024-12-02.</span>
In this machine, only O2 and N2 gases are used for processes (in PlasmaAsher1, CF4 is used as well).
The typical process parameters when operating the equipment:
*Photeresist stripping
Pressure: 0.8 - 1.0 mbar
Gas: O2
Power: 600 - 1000 watts
Time: 5 -30 min., depending on photoresist type and thickness
A typical process time for stripping of 1.5 um AZ5214e resist is 25 min for 6 wafers load in a boat, recipe 18.
A Descum process in manual mode: O2:70, N2:70, power:150W, time:10 min
Be sure to wait for cooling if the mashine has been used at 1000W right before.
At a load at 2 Fused silica wafers resist removed 0.01-01,5um
The other materials have not been tested yet.
The user manual, user APV, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=200 LabManager] - '''requires login'''
===Process Information===
*[[Specific Process Knowledge/Lithography/Descum|Descum]]
<br clear="all" />
<!-- TARAN 220-03-05
==III-V Plasma Asher==
[[Image:III-V_asher.jpg|300x300px|thumb|Plasma asher for removing resist on III-V samples: positioned in A-5]]
Diener Pico Plasma Asher for III-V materials.
The user manual and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=186 LabManager] - '''requires login'''
<br clear="all" />
-->
==Plasma Asher 3: Descum==
[[image:2017-03-15 13.12.45.jpg|350x350px|thumb|Plasma Asher 3: Descum is placed A-5]]
The Plasma Asher 3: Descum dedicated for resist descum i.e. removal of remains resist traces after development. It has a small chamber, so you can only load one 4 inch substrate ad time or few smaller pieces.
In this machine, only O2 and N2 gases are used for processes.
The typical process parameters when operating the equipment:
*Photeresist descum
Pressure: 0.2 - 0.8mbar
Gas: O2
Power: 50% - 100%
Time: 1 -10 min., depending on photoresist type and thickness
The other materials have not been tested yet.
The user manual, user APV, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=423 LabManager] - '''requires login'''
===Process Information===
*[[Specific Process Knowledge/Lithography/Descum|Descum]]
<br clear="all" />
<!-- TARAN 220-03-05
==III-V Plasma Asher==
[[Image:III-V_asher.jpg|300x300px|thumb|Plasma asher for removing resist on III-V samples: positioned in A-5]]
Diener Pico Plasma Asher for III-V materials.
The user manual and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=186 LabManager] - '''requires login'''
<br clear="all" />
-->
=Plasma Asher 4=
<span style="color:red">Coming soon</span>
=Plasma Asher 5=
<span style="color:red">Coming soon</span>
=Resist Strip=
[[Image:Resist_strip.jpg|300x300px|thumb|Resist strip bench in D-3]]
This resist strip is only for wafers without metal and SU-8.
There are one Remover 1165 bath for stripping and one IPA bath for rinsing.
'''Here are the main rules for resist strip use:'''
*Place the wafers in a wafer holder and put them in the first bath for 10 min, this time is depending how much resist you have on the surface.
*After the strip rinse your wafers in the IPA bath for 2-3 min.
*Rinse your wafers for 4-5 min. in running water after stripping.
The user manual and contact information can be found in LabManager: [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=385 Resist Strip] - '''requires login'''
[[Specific Process Knowledge/Lithography/Strip/PlasmaAsher2|Information about decommissioned tool can be found here.]]
Plasma Asher 3: Descum is a low power plasma asher dedicated for descumming on smaller substrates.
Product name: Diener Pico Plasma Asher
Year of purchase: 2014
The Plasma Asher 3: Descum is dedicated for resist descum, i.e. removal of remains resist traces after development. It has a small chamber, so you can only load a single 100 mm substrate, or a few smaller pieces.
In this machine, only Oxygen is used for processing.
Typical process parameters:
Process: Photoresist descumming
Pressure: 0.2-0.8 mbar
Gas: 45 sccm O2
Power: 100 W (100%)
Time: 1 -10 minutes (depending on photoresist type and thickness)
Other materials have not been tested.
The user manual, user APV, and contact information can be found in LabManager - requires login
Process Information
Detailed information about descum processing on Plasma asher 3: Descum can be found here.
Plasma Asher 4
Plasma asher 4 in cleanroom E-5.
Product name: PVA Tepla Gigabatch 380M
Year of purchase: 2024
The Plasma Asher 4 can be used for the following processes:
Photoresist stripping
Descumming
Surface cleaning
Removal of organic passivation layers and masks
Plasma asher 4 has the following material restrictions:
No metals allowed
No metal oxides allowed
No III-V materials allowed
The user manual, risk assessment, and contact information can be found in LabManager - requires login
Typical stripping parameters
Tested with 1.5 µm AZ 5214E on 100 mm silicon substrate.
Product name: PVA Tepla Gigabatch 380M
Year of purchase: 2024
The Plasma Asher 5 can be used for the following processes:
Photoresist stripping
Descumming
Surface cleaning
Removal of organic passivation layers and masks
Furthermore plasma processing using CF4 in plasma asher 5 can be used for:
Etching of glass and ceramic
Etching of SiO2, Si3N4, Si
Removal of polyimide layers
Plasma asher 5 can be used for almost every material, but if you have any doubt if your materials are compatible/allowed in plasma asher 5, feel free to ask the lithography group at Nanolab.
The user manual, risk assessment, and contact information can be found in LabManager - requires login
Process Information
Plasma asher 5 is identical to plasma asher 4, see resist strip processing for plasma asher 4 here.
In the resist strip it is allowed to strip resist that is deposited on a metal layer. It is not allowed to strip resist with metal on top (lift off). Furthermore no SU-8 is allowed in the bath.
There are one Remover 1165 bath for stripping and one IPA bath for rinsing.
Here are the main rules for resist strip use:
Place the wafers in a wafer holder and put them in the first bath for 10 min, this time is depending how much resist you have on the surface.
After the strip rinse your wafers in the IPA bath for 2-3 min.
Rinse your wafers for 4-5 min. in running water after stripping.
The user manual and contact information can be found in LabManager: Resist Strip - requires login