Jump to content

Specific Process Knowledge/Thin film deposition/thermalevaporator: Difference between revisions

From LabAdviser
Mdyma (talk | contribs)
Created page with "=<span style="background:#FF2800">THIS PAGE IS UNDER CONSTRUCTION</span>200px= '''Feedback to this page''': '''[mailto:pvd@danchip.dtu.dk?Sub..."
 
Reet (talk | contribs)
No edit summary
 
(92 intermediate revisions by 5 users not shown)
Line 1: Line 1:
=<span style="background:#FF2800">THIS PAGE IS UNDER CONSTRUCTION</span>[[image:Under_construction.png|200px]]=
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Thin_film_deposition/thermalevaporator click here]'''


'''Feedback to this page''': '''[mailto:pvd@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php?title=Specific_Process_Knowledge/Thin_film_deposition/Alcatel&action=edit click here]'''
<i> This page is written by <b>DTU Nanolab staff</b></i>


[[Category: Equipment|Thin film]]
[[Category: Equipment|Thin film]]
[[Category: Thin Film Deposition|Alcatel]]
[[Category: Thin Film Deposition|Thermal Evaporator]]




==Alcatel - A system for deposition of metals==
==Thermal evaporator for metal deposition==
[[Image:Alcatel.jpg|300x300px|thumb| positioned in cleanroom A-1.]]
[[Image:IMG_2592_edit.jpg|300x300px|thumb| Positioned in cleanroom A-1.]]


This instrument is NANO 36 Thermal evaporator from Kurt J. Lesker. Instrument specifications below. It takes around 1 hour for a round of deposition (depending on thickness and rate of course). The small chamber means that the deposited thickness may vary quite a bit across large samples, as further described in the specifications table.


The main purpose of this evaporator is to deposit Al for dissipation of charge when doing electron beam lithography on insulating substrates. It can also be used for Cr evaporation for the same purpose. The advantage of Al is that it can be removed simultaneously with the e-beam resist. However Cr may allow even better resolution of the lithography.


Additionally we have processes for evaporation of Ag, Au, Cu, and Ge. We have also attempted to evaporate Zn, but this resulted in heavy contamination of the chamber. You are always welcome to ask for other metals in the machine.


'''The user manual, quality control procedure and results, user APV, technical information and contact information can be found in LabManager:'''  
Up to two sources can be present at the same time (metals in a boat, crucible or rod for evaporation) but there is only one power supply, so only one material can be evaporated at a time.
 
'''The user manual, APV, technical information, cross-contamination sheet and contact information can be found in LabManager:'''  
<!-- remember to remove the type of documents that are not present -->
<!-- remember to remove the type of documents that are not present -->


<!-- give the link to the equipment info page in LabManager: -->
<!-- give the link to the equipment info page in LabManager: -->
[http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=20 Alcatel in LabManager]
[http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=404 Thermal Evaporator in LabManager]


<br clear="all" />
<br clear="all" />


==Process information==
==Process information==
====Materials for e-beam evaporation====
====Materials evaporated in the Lesker Thermal Evaporator====


*[[Specific Process Knowledge/Thin film deposition/Deposition of Aluminium|Aluminium (Al)]]
*[[Specific Process Knowledge/Thin film deposition/Deposition of Aluminium/Thermal deposition of Al|Aluminium]]
*[[Specific Process Knowledge/Thin film deposition/Deposition of Chromium|Chromium (Cr)]]
*[[Specific Process Knowledge/Thin film deposition/Deposition of Silver/Deposition of Silver in Thermal Evaporator|Silver]]
*[[Specific Process Knowledge/Thin film deposition/Deposition of Copper|Copper (Cu)]]
*[[Specific Process Knowledge/Thin film deposition/Deposition of Chromium/Thermal evaporation of Cr in Thermal evaporator|Chromium]]
*[[Specific Process Knowledge/Thin film deposition/Deposition of Gold|Gold (Au)]]
*[[Specific Process Knowledge/Thin film deposition/Deposition of Germanium/Thermal Ge evaporation Thermal Evaporator|Germanium]]
*[[Specific Process Knowledge/Thin film deposition/Deposition of Molybdenum|Molybdenum (Mo)]]
*[[Specific Process Knowledge/Thin film deposition/Deposition of Gold/Resistive thermal evaporation of Au in Thermal Evaporator|Gold]]
*[[Specific Process Knowledge/Thin film deposition/Deposition of Nickel|Nickel (Ni)]]
*[[Specific Process Knowledge/Thin film deposition//Deposition of Copper/Resistive thermal evaporation of Copper|Copper]]
*[[Specific Process Knowledge/Thin film deposition/Deposition of Palladium|Palladium (Pd)]]
*([[Specific Process Knowledge/Thin film deposition/Deposition of Zinc|Zinc]] - we don't like to evaporate this material)
*[[Specific Process Knowledge/Thin film deposition/Deposition of Platinum|Platinum (Pt)]]
*[[Specific Process Knowledge/Thin film deposition/Deposition of Silver|Silver (Ag)]]
*[[Specific Process Knowledge/Thin film deposition/Deposition of Tantalum|Tantalum (Ta)]]
*[[Specific Process Knowledge/Thin film deposition/Deposition of Tin|Tin (Sn)]]
*[[Specific Process Knowledge/Thin film deposition/Deposition of Titanium|Titanium (Ti)]] 
*[[Specific Process Knowledge/Thin film deposition/Deposition of Tungsten|Tungsten (W)]] - thinner layers


We can develop processes for other materials if requested.


==Equipment performance and process related parameters Alcatel==
==Equipment performance and process related parameters==


{| border="2" cellspacing="0" cellpadding="10"  
{| border="2" cellspacing="0" cellpadding="10"  
|-
|-
!style="background:silver; color:black;" align="left"|Purpose  
!style="background:silver; color:black;" align="left"|Purpose  
|style="background:LightGrey; color:black"|Deposition of metals and silicon ||style="background:WhiteSmoke; color:black"|
|style="background:LightGrey; color:black"|Deposition of metals ||style="background:WhiteSmoke; color:black"|
*E-beam evaporation of metals
*Thermal evaporation of metals
*Sputtering of Silicon
|-
|-
!style="background:silver; color:black" align="left" valign="top" rowspan="2"|Performance
!style="background:silver; color:black" align="left" valign="top" rowspan="5"|Performance
|style="background:LightGrey; color:black"|Film thickness||style="background:WhiteSmoke; color:black"|
|style="background:LightGrey; color:black"|Film thickness||style="background:WhiteSmoke; color:black"|
*10Å - 1µm* (for some materials)
*10Å - 1µm (Al)
*10Å - 0.5µm (Ag)
*up to 100 nm (Cr)
*ask the [mailto:thinfilm@nanolab.dtu.dk Thin Film group] if in doubt or if you wish to exceed the limits
|-
|-
|style="background:LightGrey; color:black"|Deposition rate
|style="background:LightGrey; color:black"|Deposition rate
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*2Å/s - 15Å/s
*0.5-2 Å/s (Al), 5 Å/s (Ag), 1 Å/s (Cr)
*In general, 0.5-10 Å/s is possible
*We need to develop a new process for each rate
|-
|style="background:LightGrey; color:black"|Thickness uniformity ('''no rotation''', wafer centered above source)*
|style="background:WhiteSmoke; color:black"|
*Approx. 6-9 % variation on a 4" wafer with 100 nm Al (crucible source)
*Approx. 8-13 % variation on a 6" wafer with 100 nm Al (crucible source)
*Approx. 23 % variation on a 4" wafer with 100 nm Ag (boat source) - expect better result with rotation
*Approx. 10 % variation on a 6" wafer with 100 nm Cr (rod source)
|-
|style="background:LightGrey; color:black"|Thickness uniformity ('''with rotation''')
|style="background:WhiteSmoke; color:black"|
*Approx. 6-9 % Wafer-in-Wafer variation on 4" wafers with Al (crucible source) using 3-wafer holder (4 % variation wafer-to-wafer)
*Approx. 6 % variation for 6" wafers with Al (crucible source) with wafer off-center on holder
*Approx. 7 % variation for 6" wafers with Al (crucible source) with wafer centered on holder
|-
|style="background:LightGrey; color:black"|Pumpdown time
|style="background:WhiteSmoke; color:black"|
 
*about 15-25 min
|-
|-
!style="background:silver; color:black" align="left" valign="top" rowspan="2"|Process parameter range
!style="background:silver; color:black" align="left" valign="top" rowspan="2"|Process parameter range
Line 63: Line 85:
|style="background:LightGrey; color:black"|Process pressure
|style="background:LightGrey; color:black"|Process pressure
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
* Low than 4*10<sup>-6</sup> mbar
* Below 4*10<sup>-6</sup> mbar
|-
|-
!style="background:silver; color:black" align="left" valign="top" rowspan="3"|Substrates
!style="background:silver; color:black" align="left" valign="top" rowspan="3"|Substrates
|style="background:LightGrey; color:black"|Batch size
|style="background:LightGrey; color:black"|Batch size
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*One 4" wafer per run
*Up to 1 x 6 " or 8" wafer
*Or several smaller pieces
*Up to 3 x 4" wafers
*Many smaller pieces
*Deposition on one side of the substrate
*Deposition on one side of the substrate
|-
|-
Line 88: Line 111:
|-  
|-  
|}
|}
''*'' ''The variation is defined as (Max-Min)/Average for the various points measured on the wafer. The max. point was around the center and the min. somewhere along the edge. The exact location of the maximum thickness depends how the sample is placed relative to the point of maximum material flux. 
''Number for Al 4" no rotation based on QC measurements 2018-2023.


'''*''' ''For thicknesses above 200 nm permission is requested.''
''Other measurements by Rebecca Ettlinger, Evgeniy Shkondin and Patama Pholprasit 2018-2023''

Latest revision as of 12:01, 18 June 2025

Feedback to this page: click here

This page is written by DTU Nanolab staff


Thermal evaporator for metal deposition

Positioned in cleanroom A-1.

This instrument is NANO 36 Thermal evaporator from Kurt J. Lesker. Instrument specifications below. It takes around 1 hour for a round of deposition (depending on thickness and rate of course). The small chamber means that the deposited thickness may vary quite a bit across large samples, as further described in the specifications table.

The main purpose of this evaporator is to deposit Al for dissipation of charge when doing electron beam lithography on insulating substrates. It can also be used for Cr evaporation for the same purpose. The advantage of Al is that it can be removed simultaneously with the e-beam resist. However Cr may allow even better resolution of the lithography.

Additionally we have processes for evaporation of Ag, Au, Cu, and Ge. We have also attempted to evaporate Zn, but this resulted in heavy contamination of the chamber. You are always welcome to ask for other metals in the machine.

Up to two sources can be present at the same time (metals in a boat, crucible or rod for evaporation) but there is only one power supply, so only one material can be evaporated at a time.

The user manual, APV, technical information, cross-contamination sheet and contact information can be found in LabManager:

Thermal Evaporator in LabManager


Process information

Materials evaporated in the Lesker Thermal Evaporator

We can develop processes for other materials if requested.

Equipment performance and process related parameters

Purpose Deposition of metals
  • Thermal evaporation of metals
Performance Film thickness
  • 10Å - 1µm (Al)
  • 10Å - 0.5µm (Ag)
  • up to 100 nm (Cr)
  • ask the Thin Film group if in doubt or if you wish to exceed the limits
Deposition rate
  • 0.5-2 Å/s (Al), 5 Å/s (Ag), 1 Å/s (Cr)
  • In general, 0.5-10 Å/s is possible
  • We need to develop a new process for each rate
Thickness uniformity (no rotation, wafer centered above source)*
  • Approx. 6-9 % variation on a 4" wafer with 100 nm Al (crucible source)
  • Approx. 8-13 % variation on a 6" wafer with 100 nm Al (crucible source)
  • Approx. 23 % variation on a 4" wafer with 100 nm Ag (boat source) - expect better result with rotation
  • Approx. 10 % variation on a 6" wafer with 100 nm Cr (rod source)
Thickness uniformity (with rotation)
  • Approx. 6-9 % Wafer-in-Wafer variation on 4" wafers with Al (crucible source) using 3-wafer holder (4 % variation wafer-to-wafer)
  • Approx. 6 % variation for 6" wafers with Al (crucible source) with wafer off-center on holder
  • Approx. 7 % variation for 6" wafers with Al (crucible source) with wafer centered on holder
Pumpdown time
  • about 15-25 min
Process parameter range Process Temperature
  • Approximately room temperature
Process pressure
  • Below 4*10-6 mbar
Substrates Batch size
  • Up to 1 x 6 " or 8" wafer
  • Up to 3 x 4" wafers
  • Many smaller pieces
  • Deposition on one side of the substrate
Substrate material allowed
  • Silicon wafers
  • Quartz wafers
  • Pyrex wafers
Material allowed on the substrate
  • Silicon oxide
  • Silicon (oxy)nitride
  • Photoresist
  • PMMA
  • Mylar
  • Metals

* The variation is defined as (Max-Min)/Average for the various points measured on the wafer. The max. point was around the center and the min. somewhere along the edge. The exact location of the maximum thickness depends how the sample is placed relative to the point of maximum material flux.

Number for Al 4" no rotation based on QC measurements 2018-2023.

Other measurements by Rebecca Ettlinger, Evgeniy Shkondin and Patama Pholprasit 2018-2023