SiO2 can be etched in the Plasma Asher using CF4
Test work done January 2014 by Lis Nielsen and Berit Herstrøm @Nanolab
SiO2 can be etched in the Plasma Asher using CF4 and aluminum as a masking material. This gives an isotropic etch. In test2 the SiO2 layer has been etched through and there is a small over etch in the Silicon substrate. The masking material is 100 nm Al. Etch rate and uniformity measurements have been done on wafers with no mask.
- Images of isotropic SiO2 etch in the Plasma asher: Test 2
-
Profile image - a little rotated
-
Profile image
-
Tilted profile image of lines
-
Tilted profile image of lines