Development Comparison Table

Manual beaker development Developer: SU8 (Wet bench) Developer: E-beam 02 Developer: TMAH Manual 02 Developer: TMAH UV-lithography Developer: TMAH Stepper
Purpose

Fall-back option if you have a process, which is not compatible with the automatic, or semi-automatic, tools

Requires individual risk assessment for TMAH development!

Development of:

  • SU-8

Development of:

  • ZEP 520A
  • AR-P 6200.xx (CSAR)

Development of:

  • AZ nLOF
  • AZ MiR 701
  • AZ 5214E
  • AZ 4562
  • DUV resists

Development of:

  • AZ nLOF
  • AZ MiR 701
  • AZ 5214E
  • AZ 4562
  • DUV resists

Post-exposure baking

Development of:

  • DUV resists

Post-exposure baking

Developer Process dependent mr-Dev 600 (PGMEA)
  • ZED N-50
  • AR 600-50
AZ 726 MIF (2.38% TMAH in water) AZ 726 MIF (2.38% TMAH in water) AZ 726 MIF (2.38% TMAH in water)
Method Submersion Submersion Puddle Puddle Puddle Puddle
Handling

Manual handling in beakers

  • Chip bucket
  • Single wafer carrier
  • Carrier for up to 5 wafers
  • Chip bucket
  • Single wafer carrier
  • Carrier for up to 6 wafers
  • Vacuum-free edge-grip chucks for 50 mm, 100 mm & 150 mm, and 200 mm substrates
  • Chip chuck for chips & 50 mm substrates
  • Vacuum-free edge-grip chuck for 100 mm & 150 mm substrates
  • Chip chuck for chips & 50 mm substrates
Vacuum chuck Vacuum chuck
Process temperature Room temperature Room temperature Room temperature Room temperature Room temperature Room temperature
Process agitation No agitation allowed Magnetic stirrer Rotation Rotation Rotation Rotation
Process rinse Process dependent IPA IPA DI water DI water DI water
Substrate size
  • Chips
  • 50 mm wafers
  • 100 mm wafers
  • 150 mm wafers
  • Chips
  • 50 mm wafers
  • 100 mm wafers
  • 150 mm wafers
  • 200 mm wafers
  • Chips (5mm to 2")
  • 50 mm wafers
  • 100 mm wafers
  • 150 mm wafers
  • 200 mm wafers
  • Chips (5mm to 50 mm)
  • 100 mm wafers
  • 150 mm wafers
  • 100 mm wafers
  • 150 mm wafers
  • 200 mm wafers (may require tool change)
  • 100 mm wafers
  • 150 mm wafers
  • 200 mm wafers (may require tool change)
Allowed materials All cleanroom approved materials
  • Silicon and glass substrates
  • Film or pattern of all but Type IV
All cleanroom approved materials
  • All cleanroom approved materials
  • Film or pattern of all types
  • Silicon and glass substrates
  • Films, or patterned films, of any material except type IV (Pb, Te)
  • Silicon, III-V, and glass substrates
  • Films, or patterned films, of any material except type IV (Pb, Te)
Batch size 1 - 5 1 - 6 1 1 1 - 25 1 - 25






Manual beaker development in fumehood

Beaker development, in fume hood 09: UV development or fume hood 10: e-beam development, is a fall-back option if you have a process, which is not compatible with the automatic, or semi-automatic, tools. We always recommend using, or at least trying, the automatic and semi-automatic tools, instead of using manual beaker development.

Manual beaker development is necessary for some processes, but should be avoided if possible, due to the fact that it is notoriously difficult to get a stable repeatable process - especially when multiple users are sharing the same process; everybody simply does things a bit different from each other, which leads to changes in the process outcome. Some processes have a very narrow process window, which makes them inherently sensitive to small changes in the development. The manual development also has a much greater chance of producing particles, both from the operator and the environment.

Finally the safety of the operator is at a significantly higher risk, since any manual handling of chemicals carries the risk of accidental spills with it. This is especially problematic if the developer is TMAH based, where direct skin exposure of >1% TMAH on a few percent of the body must be treated as a life-threatening event.

Special rules for manual beaker development of TMAH

  • Automatic agitation methods are not allowed - this includes magnetic stirring or sonication
  • Manual agitation methods, which create large waves or turbulence in the development solution, are not allowed
  • Users must submit a risk assessment for any process requiring manual beaker development of TMAH based developers
  • Users requiring manual beaker development of TMAH based developers must additionally provide valid reasons for not using the already available automatic and semi-automatic tools

Standard manual beaker development procedure

Standard procedure for manual beaker development in fume hood:
1) Submerge exposed substrate into development solution
2) When timer ends, move substrate directly into Rinse 1
3) After a few seconds, move substrate into Rinse 2*
4) Remove developed substrate for drying
(*It is allowed to omit the Rinse 2 step)

The standard procedure for manual beaker development in a fume hood is as follows:

  1. Prepare development process
  2. Perform development
  3. Clean up

Prepare development process

  • Write the chemical label, which must always be present in your chemical setup - your write your label before pouring the chemical
  • Find the beakers required for your process
  • Find the items required for holding/submerging your substrate during the process
  • Find carriers or other storage units for placing your substrate after the process has finished
  • Find a timer - make sure it works as you expect it to, before submerging your substrate into the development solution and discovering that the timer is in fact broken
  • Get some cleanroom wipes and keep them nearby, for wiping any drops spilled during handling
  • Do not cover too many of the exhaust holes in the fume hood table, as this will reduce the efficiency of the exhaust, which reduces safety
  • Do not place your beakers too close to the fume hood sash, as this can make it difficult to efficiently extract the fumes escaping from the beakers, which reduces safety

Perform development

  1. Put on the appropriate personal protection gear
  2. Pour rinsing agent into Rinse 1 and Rinse 2 beakers - typically DI water or IPA
  3. Pour development solution into development beaker
  4. Place exposed substrate in the appropriate carrier
  5. Set timer
  6. Submerge substrate into development beaker
  7. Start timer immediately
  8. When timer is 5 seconds from ending, prepare to lift the substrate out of the development beaker
  9. Lift substrate out of development beaker - it can help to lift it at a slight angle, to allow liquids to drain more easily from large surfaces
  10. Submerge it immediately into Rinse 1
  11. Agitate up/down for at least a few seconds
  12. Move substrate into Rinse 2*
  13. Agitate slightly
  14. The developed substrate can now be removed and dried

(*It is allowed to omit the Rinse 2 step)

Clean up

  • Pour Rinse 1 and Rinse 2 into appropriate waste: water goes into the sink, IPA goes into C-waste drain
  • Rinse beakers with the DI-water gun
  • Pour development solution into appropriate waste: solvent based developer goes into C-waste drain. NB! TMAH is an aqueous alkaline solution, which must never be mixed with solvents! TMAH waste goes into the dedicated TMAH waste container, stored in the chemical cabinet in E-4.
  • If your developer solution is not TMAH based:
    • Rinse beaker 3 times, discard water into sink
  • If your developer solution is TMAH based:
    • Rinse beaker once with DI-water and discard this into the TMAH waste
    • Rinse beaker two more times, discarding the water into the sink
  • Hang all beakers to dry on the drying rack
  • Erase the chemical label text
  • Wipe any droplets on the fume hood surface
  • Discard any napkins/other trash in the bin inside the fume hood


Developer: SU8 (Wet Bench)

The Developer: SU8 (Wet Bench) is located in E-4.

Tool description
The Developer: SU-8 (wet bench) is a manually operated wet bench for submersion development of SU-8 photoresist in PGMEA (supplied in the cleanroom as the product mr-Dev 600).

The SU-8 development is a three-stage process:

  1. Submerge into "FIRST" bath to dissolve the bulk of the resist
  2. Submerge into "FINAL" bath to finish the development
  3. Submerge into "RINSE" bath to stop the development process and rinse the substrates

The development time is controlled manually by the user. After development the substrates are dried in the empty bath, which is dedicated for drying.

Product: Arias wet bench
Year of purchase: 2023
Location: Cleanroom E-4

User manual
The user manual and contact information can be found in LabManager - requires login

Tool training
Training on the tool requires users to complete the lithography TPT followed by online tool training and hands-on authorization training.

Equipment performance and process related parameters

Tool purpose

Development of:

  • SU-8
Developer mr-Dev 600 (PGMEA)
Development method Submersion
Handling method Multi- or single wafer holder
Process temperature Room temperature
Process agitaion Magnetic stirrer
Process rinse IPA
Substrate sizes
  • Chips
  • 50 mm wafers
  • 100 mm wafers
  • 150 mm wafers, check the liquid level in the baths
  • 200 mm wafer, check the liquid level in the baths
Substrate materials
  • Silicon and glass substrates
  • Film, or pattern, of all materials except Type IV
Substrate batch size 1-6


Process information

Several aspects of the SU-8 processing outcome are affected by the development process:

  • The lithographic resolution is affected by the time between PEB (post-exposure bake) and development, as the cross-linking process continues in the interface between exposed and unexposed regions even at room temperature
  • Cracks in the structures is affected by two things; the development time, and how much has previously been developed in the developer bath. Cracking is worse with longer development time, and worse in a fresh developer bath. This effect of the developer quickly saturates after developing 5-10 wafers
  • The stability of fine structures (high aspect ratio structures) is affected by the rinse after development, as the lower surface tension of IPA compared to PGMEA reduces pattern collapse during drying


Development time
Development time is strongly dependent on the SU-8 thickness:

  • Minimum development time: 1 min per 20 µm in FIRST bath
  • Maximum development time: SU-8 is not very sensitive to over-development


Recommendations for development time:

  • ≤5 µm: 2 minutes in FIRST bath, followed by 2 minutes in FINAL bath
  • ~40 µm: 5 minutes in FIRST bath, followed by 5 minutes in FINAL bath
  • ≥180 µm: 15 minutes in FIRST bath, followed by 15 minutes in FINAL bath

Developer: E-beam 02

Developer: E-beam 02 is located in E-4.

Tool description
The Developer: E-beam 02 is a semi-automatic and programmable single substrate developer system, which can be used for development of resists on chips, 50 mm, 100 mm, 150 mm and 200 mm substrates. The development is done using ZED-N50 or AR 600-50 developers and IPA for rinsing.

Single substrates are loaded manually into the tool, but the developer dispense, puddle time, agitation, rinse and drying is controlled by the tool.

Product: Laurell EDC-650Hz-8NPPB-IND
Year of purchase: 2024
Location: Cleanroom E-4

User manual
The user manual and contact information can be found in LabManager - requires login

Tool training
Training on the tool requires users to complete the lithography TPT followed by the online tool training and a hands-on authorization training.
The tool training video is part of the online tool training, but can also be viewed here (the video is for Developer: TMAH Manual 02, but the two tools are almost identical).

Equipment performance and process related parameters

Tool purpose

Development of:

  • AR-P 6200.xx (CSAR)
  • ZEP 520
  • Other E-beam resists
Developer
  • AR 600-50
  • ZED N-50
Development method Puddle
Handling method
  • Non-vacuum chuck for 200 mm wafers
  • Non-vacuum chuck for 100 mm & 150 mm wafers
  • Non-vacuum chuck for 50 mm wafers
  • Non-vacuum chuck for chips
Process temperature Room temperature
Process agitaion 4 cycles per minute
Process rinse IPA
Substrate sizes
  • Chips
  • 50 mm wafers
  • 100 mm wafers
  • 150 mm wafers
  • 200 mm wafers
Substrate materials
  • All cleanroom allowed materials
  • Film, or pattern, of all materials except Type IV
Substrate batch size 1


Process information

All recipes use the following structure:

  1. Pressurize the developer canister
  2. Dispense puddle while rotating substrate slowly
  3. Puddle development with/without agitation of substrate
  4. Spin off developer
  5. Clean substrate with IPA
  6. Dry substrate and chamber with nitrogen


Multi puddle
Multi puddle recipes repeat steps 2-4 for the given number of puddles.

Process recipes

(Updated 2026-01-14, JEHEM)

N50 recipes have the letter "N" in them. AR-600-50 recipes have the letter "A" in them. The number is the development time in seconds:

  • 01 Rinse
  • 02 N 15
  • 03 N 30
  • 04 N 60
  • 05 N 90
  • 06 N 120
  • 07 N 180
  • 08 N 300
  • 09 N 600
  • 10 N 2x60
  • 11 N 5x60
  • 12 A 15
  • 13 A 30
  • 14 A 60
  • 15 A 90
  • 16 A 120
  • 17 A 180
  • 18 A 300
  • 19 A 600
  • 20 A 2x60
  • 21 A 5x60
  • 30 N 3x60s
  • NILT AR
  • NILT MOE
  • NILT p30
  • NILT p31
  • NILT p32

Agitation

4 cycles per minute, 30 rpm, 30 rpm/s.

Developer: TMAH Manual 02

Developer: TMAH Manual 02 is located in E-4.

Tool description
The Developer: TMAH manual 02 is a semi-automatic and programmable single substrate developer system, which can be used for development of resists on chips, 50 mm, 100 mm and 150 mm substrates. The development is done using AZ 726 MIF, which is a 2.38% TMAH solution with wetting agent.

Single substrates are loaded manually into the tool, but the developer dispense, puddle time, agitation, rinse and drying is controlled by the tool.

Product Laurell EDC-650-HZB-23NP
Year of purchase 2016
Tool modification

Converted from e-beam solvent developer to UV TMAH developer in 2024
Added media flow controllers for developer, rinse and drying media in 2025

Location Cleanroom E-4

User manual
The user manual and contact information can be found in LabManager - requires login

Tool training
Training on the tool requires users to complete the lithography TPT followed by the online tool training and a hands-on authorization training.
The tool training video is part of the online tool training, but can also be viewed here.

Equipment performance and process related parameters

Tool purpose

Development of UV resists:

  • AZ nLOF 2020
  • AZ MIR 701
  • AZ 5214E
  • AZ 4562

Development of DUV resists:

  • KrF M230Y
  • KrF M35G
Developer AZ 726 MIF (2.38% TMAH)
Development method Puddle
Handling method
  • Non-vacuum chuck for 100 mm & 150 mm wafers
  • Non-vacuum chuck for chips and 50 mm wafers
Process temperature Room temperature
Process agitaion 15 cycles per minute
Process rinse DI water
Substrate sizes
  • Chips
  • 50 mm wafers
  • 100 mm wafers
  • 150 mm wafers
Substrate materials
  • All cleanroom allowed materials
  • Film, or pattern, of all materials except Type IV
Substrate batch size 1



Process information

All recipes use the following structure:

  1. Pressurize the TMAH canister
  2. Dispense puddle while rotating substrate slowly
  3. Puddle development with agitation of substrate
  4. Spin off developer
  5. Clean substrate and chamber with DI water
  6. Dry substrate and chamber with nitrogen


Multi puddle
Multi puddle recipes repeat steps 2-4 for the given number of puddles.

Process recipes

(Updated 2026-01-12, JEHEM)

  • -Rinse-
  • 1x015s
  • 1x030s
  • 1x060s
  • 1x120s
  • 2x060s
  • 5x060s

Agitation

Testing showed that adding agitation to the puddle step gave better uniformity in the development rate over the entire area of the substrate as well as increased development rate.

Tests were performed on under-exposed resist, specifically for showing the difference between the agitation and non-agitation puddle development - the measured results cannot necessarily be transferred directly to a working process, only the vague general behavior of the two process setups; faster/slower development speed and better/worse uniformity across substrate.

Development rate for under-exposed resist test
Non-uniformity for under-exposed resist test
Non-agitation Agitation
Test results
  • Slower development
  • Worse uniformity
  • Faster development
  • Better uniformity
Normalized development rate 1 1.20
Non-uniformity 21% 11%
Agitation None 15 cycles per minute, 20 rpm, 500 rpm/s
Substrate 100 mm SSP silicon
Resist film 1.5 µm AZ 5214E
Exposure dose 50 mJ/cm2 (~50% of normal dose)
Development Single puddle for 60 seconds
Developer AZ 726 MIF (2.38% TMAH)


Developer TMAH UV-lithography

Developer: TMAH UV-lithography is located in E-4.

Developer TMAH UV-lithography was released Q4 2014.

Link to information about developer chuck size and hotplate pin positions.

Training video


The user manual, user APV, and contact information can be found in LabManager - requires login

Process Information

Equipment performance and process related parameters

Purpose

Development of

  • AZ nLOF
  • AZ MiR 701
  • AZ 5214E
  • AZ 4562
  • DUV resists
Developer

AZ 726 MIF

(2.38% TMAH in water)

Method Development

Puddle

Handling

Vacuum chuck

Process parameters Temperature

Room temperature

Agitation

Rotation

Rinse

DI water

Substrates Substrate size
  • 100 mm wafers
  • 150 mm wafers
Allowed materials

Silicon and glass substrates

Film or pattern of all except Type IV

Batch

1-25


Developer: TMAH Stepper

The Developer-TMAH-Stepper is placed in F-3.

This developer is dedicated for development of DUV resists. The developer is fully automatic and can run up to 25 substrates in a batch 4", 6", and 8" size (8" requires tool change). The machine is equipped with 1 developer line, in our case 2,38% TMAH in water (AZ 726 MIF), 1 topside rinse line with water, 1 backside rinse line with water and 1 N2 line for drying.


The user manual and contact information can be found in LabManager - requires login


Process information

The SEM picture of 250 nm pillars and lines. Exposure dose is 140 J/m2.

The development process will be performed by the customer together with the Photolith group of DTU Nanolab. In case you would like to do DUV lithography please contact Lithography team, who will consult you and run your wafers together with you.

Here you can find a chart‎ demonstrating a dependence between 250 nm line width/pillars diameter and exposure dose.

Standard processes

Post-exposure bake sequences:

  • (1000) DCH PEB 130C 60s 60s baking at 130°C; 20s cooling
  • (1001) DCH PEB 130C 90s 90s baking at 130°C; 20s cooling

Development sequences:

  • (1004) DCH DEV 60s 60s single puddle development

Combined PEB and development sequences:

  • (1002) DCH PEB_60s and DEV_60s 60s baking at 130°C followed by 60s single puddle development
  • (1003) DCH PEB_90s and DEV_60s 90s baking at 130°C followed by 60s single puddle development

The standard developer process consists of:

  • pre-wetting with water (2.5s @ 1000rpm)
  • developer dispense (2.5s @ 40rpm, corresponding to ~9ml)
  • development (60s @ 0rpm)
  • water rinse with BSR (5s @ 3000rpm)
  • nitrogen drying (7s @ 4000rpm)

and has a cycle time of ~2 minutes


Equipment performance and process related parameters

Purpose

Development of DUV resist: KRF M230Y and KRF M35G

Developer

2,38% water based TMAH

Process parameters Spin speed

10 - 5000 rpm

Spin acceleration

100 - 10000 rpm/s

Hotplate temperature

130°C for post exposure baking

Substrates Substrate size
  • 100 mm wafers
  • 150 mm wafers
  • 200 mm wafers (requires tool change)
Allowed materials
  • Any standard cleanroom material
Batch

1 - 25