LabAdviser/Technology Research/Fabrication of Hyperbolic Metamaterials using Atomic Layer Deposition/TiO2 Q plates: Difference between revisions
| Line 1: | Line 1: | ||
====Procces flow description==== | ====Procces flow description==== | ||
A 500 μm-thick wafer of silica (SiO<sub>2</sub>) goes through RCA clean and low-pressure chemical vapor deposition (LPCVD) (furnace from Tempress) based on SiH<sub>4</sub> (silane) at 560<sup>◦</sup>C to form a layer of 300 nm of amorphous silicon (Si) [Fig. 1]. The back side of deposited Si was etched using KOH wet etch. In order to remove residues from the etching process, it was performed oxygen plasma cleaning. A deposition of 150 nm of the resist CSAR was done followed by exposure to Electron Beam Lithography (EBL) (JEOL JBX-9500 Electron-beam) [Fig. 1] generating a mask of Si with concentric ring patterns. After development, the wafer was submitted to advanced silicon etch (ASE). To form the trenches of the structures, a thin film of TiO<sub>2</sub> was deposited using the ALD technique in a hot-wall system (Picosun R200), working with 2000 cycles at 150<sup>◦</sup>C [Fig.1]. The precursors used were titanium tetrachloride (TiCl<sub>4</sub>) and H<sub>2</sub>O (supplied by Strem Chemicals Equipment). The process was followed by Ar<sup>+</sup> ion beam etching (IBE) on both sides of the wafer to remove excess[Fig. 1]. At the top most TiO<sub>2</sub> layer the physical sputtering of the sample using Ar<sup>+</sup> ions was performed in order to get access to Si core. On the backside, the Ar<sup>+</sup> ions were used to remove the deposited TiO<sub>2</sub>. Finally, we performed a reactive ion etch on silicon, leaving only the TiO<su2>2</sub> structures. The final system comprehends a base of SiO<sub>2</sub> with nano-structures of TiO<sub>2</sub> on it. Figure 2 shows the image of the system taken from scanning electron microscope (SEM) and conventional optical microscope. Figure 3 illustrates SEM cross-sectional image of the prepared q-plate. | |||
<gallery caption="" widths="1000px" heights="600px" perrow="1"> | <gallery caption="" widths="1000px" heights="600px" perrow="1"> | ||
image: | image:Q_plates_fab_sheme.jpg| Figure 1. Scheme of fabrication flow. | ||
</gallery> | </gallery> | ||
<gallery caption="" widths="1000px" heights="600px" perrow="2"> | <gallery caption="" widths="1000px" heights="600px" perrow="2"> | ||
image:TiO2nanorings.jpg| | image:TiO2nanorings.jpg| Figure 2. TiO<sub>2</sub> concentric nanorings acting as a q-plate. Insets show optical and SEM images of the whole plate. | ||
image:Q_plates_cross_section.jpg| | image:Q_plates_cross_section.jpg| Figure 3. Cross-sectional SEM image of the TiO<sub>2</sub> q-plate. | ||
</gallery> | </gallery> | ||
Revision as of 17:05, 14 March 2017
Procces flow description
A 500 μm-thick wafer of silica (SiO2) goes through RCA clean and low-pressure chemical vapor deposition (LPCVD) (furnace from Tempress) based on SiH4 (silane) at 560◦C to form a layer of 300 nm of amorphous silicon (Si) [Fig. 1]. The back side of deposited Si was etched using KOH wet etch. In order to remove residues from the etching process, it was performed oxygen plasma cleaning. A deposition of 150 nm of the resist CSAR was done followed by exposure to Electron Beam Lithography (EBL) (JEOL JBX-9500 Electron-beam) [Fig. 1] generating a mask of Si with concentric ring patterns. After development, the wafer was submitted to advanced silicon etch (ASE). To form the trenches of the structures, a thin film of TiO2 was deposited using the ALD technique in a hot-wall system (Picosun R200), working with 2000 cycles at 150◦C [Fig.1]. The precursors used were titanium tetrachloride (TiCl4) and H2O (supplied by Strem Chemicals Equipment). The process was followed by Ar+ ion beam etching (IBE) on both sides of the wafer to remove excess[Fig. 1]. At the top most TiO2 layer the physical sputtering of the sample using Ar+ ions was performed in order to get access to Si core. On the backside, the Ar+ ions were used to remove the deposited TiO2. Finally, we performed a reactive ion etch on silicon, leaving only the TiO<su2>2 structures. The final system comprehends a base of SiO2 with nano-structures of TiO2 on it. Figure 2 shows the image of the system taken from scanning electron microscope (SEM) and conventional optical microscope. Figure 3 illustrates SEM cross-sectional image of the prepared q-plate.
-
Figure 1. Scheme of fabrication flow.
-
Figure 2. TiO2 concentric nanorings acting as a q-plate. Insets show optical and SEM images of the whole plate.
-
Figure 3. Cross-sectional SEM image of the TiO2 q-plate.
Process flow
Hej Evgeniy
Jeg har lagt dette eksemple på et process flow ind. Alt tekst og billeder skal selvfølgelig erstattes af relevante process steps for denne artikel.
Mvh. Berit
| Step | Description | LabAdviser link | Image showing the step | |
|---|---|---|---|---|
| 1.1 | RCA clean | Before Si deposition in LPCVD furnace, the quartz (fused silica) wafers need to be cleaned | RCA | |
| 1.2 | LPCVD of Si | LPCVD deposition of 300 nm amorphous Si | 6" LPCVD polysilicon furnace (E2). | |
| 1.3 | Si anisotropic wet etch | Removal of the Si from the back side of the wafer. | KOH. | |
| 1.4 | Plasma surface treatment | To ensure that all organic remainings are gone, wafer is treated by O2/N2 plasma. (Optional step) | ||
| 1.5 | E-beam lithography (EBL) | Spin-coating of CSAR resist to the thickness of 150 nm, followed by e-beam exposure. | ||
| 1.6 | Advanced Silicon Etching | Creating sacrificial silicon template. | ||
| 1.7 | Scanning Electron Microscopy inspection | The fabricated template inspects by SEM | ||
| 1.8 | Plasma surface treatment | To ensure that all organic remainings are gone, template is treated by O2/N2 plasma. (Optional step) | ||
| 1.9 | Atomic Layer Deposition of TiO2 | Deposition carried at 150C.Thickness is approx. 90 nm. | Equipment used: ALD Picosun R200. Standard recipe used: TiO2T . | |
| 1.10 | Ion beam etching (IBE). | Opening of deposited TiO2 top layer using recipe "Ti acceptance" there the stage was placed to 0o degree. The back side of the wafer also needs to be exposed to etching. | IBE/IBSD Ionfab 300 | |
| 1.11 | Scanning Electron Microscopy inspection | SEM inspection of ALD deposition and IBE etching. | ||
| 1.12 | Selective etch of Si between ALD TiO2 coatings. | Si etching proceeds using Reactive Ion Etching (RIE) with isotropic process based on SFf process gas. | Equipment used: RIE2. | |
| 1.13 | Scanning Electron Microscopy inspection of fabricated structure. | Proof of final result. | ||