Specific Process Knowledge/Lithography/Coaters/Spin Coater: RCD8 processing: Difference between revisions
| Line 98: | Line 98: | ||
*'''1 TMPLT man disp Gyrset sprd''' | *'''1 TMPLT man disp Gyrset sprd''' | ||
Gyrset down; spread step; spin-off; deceleration; Gyrset up. | Gyrset down; spread step; spin-off; deceleration; Gyrset up. | ||
<!-- | |||
==Automatic dispense templates== | ==Automatic dispense templates== | ||
*'''1 TMPLT aut disp SU8''' | *'''1 TMPLT aut disp SU8''' | ||
| Line 112: | Line 112: | ||
*'''1 TMPLT aut disp Gyrset sprd''' | *'''1 TMPLT aut disp Gyrset sprd''' | ||
Dispense; Gyrset down; spread step; spin-off; deceleration; Gyrset up. | Dispense; Gyrset down; spread step; spin-off; deceleration; Gyrset up. | ||
--> | |||
=Processing results= | =Processing results= | ||
Revision as of 14:59, 27 August 2025
Specific Process Knowledge/Lithography/authors generic
Feedback to this page: click here
Spin coating
Spin coating on Spin Coater: RCD8 consists of a selection of the following steps:
- Optional: Acceleration to a low spin speed if dynamic dispense is used
- Resist dispense
- Optional: Closing the Gyrset (if used)
- Optional: Resist spreading at low spin speed
- Spin-off
- Deceleration
- Opening Gyrset
The wafer is first centered on the chuck and held in place by vacuum (or pins in the case of the non-vacuum chuck). If static dispense is used, the spindle remains static during the ensuing resist dispense. In the case of dynamic dispense, the spindle is accelerated to a low spin speed before the resist is dispensed. Using too high spin speed during dispense can cause surface wetting issues, while a too low spin speed causes the resist to flow onto the backside of the wafer. The resist may be dispensed manually, or automatically using the syringe dispense system on the media arm. After dispense, a short spin at low spin speed may be used in order to spread the resist over the wafer surface before spin-off.
The spin-off cycle determines the thickness of the resist coating. The thickness is primarily a function of the spin-off speed and the spin-off time, both following an inverse power-law. The acceleration to the spin-off speed also influences the thickness, but the effect is dependent on previous steps. The spin-off is usually a simple spin at one speed, but it may be comprised of several steps at different spin speeds. After spin-off, the wafer is decelerated.
Dispense
Resist dispense on the Spin Coater: RCD8 can only be done manually, as the motorized media arm was decommissioned in 2024. Manual dispense is done by administering the resist directly onto the substrate, after it has been loaded into the machine but before the recipe has been started. It can be done by pouring the resist directly from a bottle (for thin resists such as the AZ resists or SU-8 3005) or by pushing it out of a prefilled syringe (for thick resists like SU-8 3035 and XFT 75).
The volume dispensed from a syringe may be estimated by measuring the distance the resist level is displaced during a dispense, and calculating the corresponding volume using the diameter of the syringe (23 mm). A displacement of 10 mm corresponds to a dispensed volume of 4 ml. This calculation can also be used to mark the syringe with appropriately spaced guide lines in order to dispense a specific volume.
Tips and tricks for dispensing thick resist
High viscosity resists, such as the SU-8 formulations for coating thicknesses 50µm and above, are difficult to dispense. To have any kind of control, they require use of a dispense syringe.
Filling the syringe:
Syringes should be filled the day before spin coating, and should be stored vertical in order to allow bubbles to settle at the top.
Dispensing from the syringe:
Recipes
Auxiliary recipes, and template recipes. For each case a list of the steps/parameters in the respective recipe.
Process recipes developed by Nanolab are listed under Process results.
Auxiliary recipes
- 1 DCH Centering test
5s @ 100rpm; 5s @ 250rpm; 5s @ 500rpm.
- 1 DCH Chuck cleaning
10s @ 100rpm; 1s @ 0rpm; 10s @ -30rpm; 20s @ 1500rpm.
- 1 DCH Gyrset cleaning
Gyrset down; 10s @ 100rpm; 1s @ 0rpm; 10s @ -30rpm; 20s @ 1500rpm; Gyrset up.
- 1 DCH predispense
0.2s dispense at cup (arm position 0mm).
Manual dispense templates
- 1 TMPLT man disp
Spin-off; deceleration.
- 1 TMPLT man disp spread
Spread step; spin-off; deceleration.
- 1 TMPLT man disp Gyrset
Gyrset down; spin-off; deceleration; Gyrset up.
- 1 TMPLT man disp Gyrset sprd
Gyrset down; spread step; spin-off; deceleration; Gyrset up.
Processing results
SU-8 2075


Spin coating of SU-8 2075 on Spin Coater: RCD8 using automatic dispense consists of three process steps: static dispense, spread, and spin-off. In the static dispense step the media arm is moved to the center of the wafer, and resist is dispensed for 7s, yielding a volume of 3.5ml at 2.0 bar. After the dispense, the media arm is moved up and down in a series of steps designed to break the string of resist between the syringe and the wafer. In the spread step the wafer is accelerated to 700rpm at 50rpm/s, and spun for 25s. In the spin-off step the wafer is accelerated at 500rpm/s to the spin-off speed, spun for 30s, then decelerated at 1000rpm/s.
In the Gyrset version, the Gyrset is closed after the dispense step, and opened after the spin-off step.
Recipe names, process parameters, and test results:
- 1 DCH SU8 aut disp 100um
Spin-off: 30 s at 2100 rpm.
| Substrate | Thickness | Uniformity (+/-) | Test date | Tester initials | Comments |
|---|---|---|---|---|---|
| Silicon with native oxide | 100 µm | 3.5% | 14/4 2015 | taran | 5 points on one wafer, exclusion zone 15mm |
- 1 DCH SU8 aut dsp Grst 100um
Spin-off: 30 s at 2000 rpm.
| Substrate | Thickness | Uniformity (+/-) | Test date | Tester initials | Comments |
|---|---|---|---|---|---|
| Silicon with native oxide | 99 µm | 3.0% | 15/4 2013 | taran | 5 points on one wafer, exclusion zone 15mm |
AZ 4562

Spin coating of AZ 4562 on Spin Coater: RCD8 using manual dispense is a very simple process. The wafer is accelerated at 1000rpm/s to the spin-off speed, spun for 30s, then decelerated at 1000rpm/s.
Recipe names, process parameters, and test results:
- 1 DCH 4562 man disp 10um
Spin-off: 30 s at 2000 rpm.
| Substrate | Thickness | Uniformity (+/-) | Test date | Tester initials | Comments |
|---|---|---|---|---|---|
| Silicon with native oxide | 9.92 µm | 2.9% | 29/4 2015 | taran | 9 points on one wafer, exclusion zone 5mm Non-vacuum chuck |
AZ 5214E

Spin coating of AZ 5214E on Spin Coater: RCD8 using manual dispense is a very simple process. The wafer is accelerated at 1000rpm/s to the spin-off speed, spun for 30s, then decelerated at 1000rpm/s.
Recipe names, process parameters, and test results:
- 1 DCH 5214E man disp 2.2um
Spin-off: 30 s at 2100 rpm.
| Substrate | Thickness | Uniformity (+/-) | Test date | Tester initials | Comments |
|---|---|---|---|---|---|
| Silicon with native oxide | 2.19 µm | 0.4% | 22/4 2013 | taran | 9 points on one wafer, exclusion zone 5mm |
AZ MiR 701

Spin coating of AZ MiR 701 (29cps) on Spin Coater: RCD8 using manual dispense is a very simple process. The wafer is accelerated at 1000rpm/s to the spin-off speed, spun for 30s, then decelerated at 1000rpm/s.
Recipe names, process parameters, and test results:
- 1 DCH MiR 701 man disp 2um 1)
Spin-off: 30 s at 2350 rpm.
| Substrate | Thickness | Uniformity (+/-) | Test date | Tester initials | Comments |
|---|---|---|---|---|---|
| Silicon with native oxide | 2.00 µm | 1.8% | 29/4 2015 | taran | 9 points on one wafer, exclusion zone 5mm Non-vacuum chuck |
1) Not implemented yet.
AZ nLOF 2020

Spin coating of AZ nLOF 2020 on Spin Coater: RCD8 using manual dispense is a very simple process. The wafer is accelerated at 1000rpm/s to the spin-off speed, spun for 30s, then decelerated at 1000rpm/s.
Recipe names, process parameters, and test results:
- 1 DCH nLOF 2020 man disp 2.3um 1)
Spin-off: 30 s at 2500 rpm.
| Substrate | Thickness | Uniformity (+/-) | Test date | Tester initials | Comments |
|---|---|---|---|---|---|
| Silicon with native oxide | 2.30 µm | 1.7% | 29/4-2015 | taran | 9 points on one wafer, exclusion zone 5mm Non-vacuum chuck |
1) Not implemented yet.