Specific Process Knowledge/Lithography/Descum: Difference between revisions
| Line 175: | Line 175: | ||
You can use different strategy planing your descum: you can change power settings or you can vary chamber pressure during descum. | You can use different strategy planing your descum: you can change power settings or you can vary chamber pressure during descum. | ||
Testing different power settings | ''Testing different power settings'' | ||
Recipe settings: | |||
Oxydgen: 5 sccm under process | Kept oxygen and pressure settings constant at Oxydgen: 5 sccm under process; Pressure: 0,2mbar and vary power. | ||
Pressure: 0,2mbar | |||
Experiment parameters: | Experiment parameters: | ||
| Line 197: | Line 196: | ||
|} | |} | ||
''Testing different pressure settings'' | |||
Recipe settings: | |||
Kept power setting constant at Power: 100% and vary oxydgen flow during process. | |||
Experiment parameters: | |||
{| {{table}} | |||
| align="center" | | |||
{| border="1" cellspacing="1" cellpadding="2" align="center" | |||
|- style="background:LightGrey" | |||
| ||FW/REV|| C2/C1 || Oxydgen || Pressure | |||
|- | |||
|'''recipe 1'''|| 100/0 || 53/31 || 5 || 0,2 | |||
|- | |||
|'''recipe 2''' || 100/0 || 37/38 || 45 || 0,8 | |||
|- | |||
|} | |||
|} | |||
'''Ashing of AZ5214E resist''' | '''Ashing of AZ5214E resist''' | ||
Revision as of 11:32, 15 March 2022
Feedback to this page: click here
Descum results
Plasma asher 1

Descum of AZ5214E resist on 50mm silicon wafer. Wafer was placed horisontally in chamber on a 100 mm carier wafer.
Note: Plasma asher was cold before use
| ||||||||||||||||||||||||||||||||||||||||||||||||||
Conny Hjort & Jesper Hanberg September 2019

Descum of different resists, AZ5214E, AZ701 MiR and AZ2020 nLOF, on a single 100mm wafer was tested. Wafer was placed vertically in the middle of glass carrier.
Recipe setting was the same as in previous test in September 2019: 70ml/min O2, 70 ml/min N2, power 150W, different ashing time 1, 2, 3, 5 and 7 min run. Plasma Asher was cold before use, we observed minor temperature rise during processing, but not more than 5 degrees. Starting chambers pressure was around 0, 5 mbar.
1,5 um AZ5214E resist
|
1,5 um AZ5214E resist placed horizontally in the carrier
|
1,5 um AZ701MiR resist
|
1,5 um AZ 2020nLOF resist
|
Plasma asher 2

Descum of AZ Mir 701 resist on 100mm silicon wafer. Five wafers were placed vertically in chamber.
Experiment parameters:
|
recipe 1
|

recipe 2
|
We can observe linear dependance of etched material on time after etching 7 minutes and more (recipe 2).
Jitka Urbánková & Jesper Hanberg
December 2019
Plasma asher 3
Plasma Asher 3 is specially used for control descum process after lithography. Please notice that you only can process one 4 inch wafer or one small sampel ad time. Machine is equipt with 2 gaslines: oxydgen and nitrogen, but all test run with oxydgen as recommended by Diener.
Ashing of AZ MiR701 resist

You can use different strategy planing your descum: you can change power settings or you can vary chamber pressure during descum.
Testing different power settings
Recipe settings: Kept oxygen and pressure settings constant at Oxydgen: 5 sccm under process; Pressure: 0,2mbar and vary power.
Experiment parameters:
|
Testing different pressure settings
Recipe settings: Kept power setting constant at Power: 100% and vary oxydgen flow during process.
Experiment parameters:
|
Ashing of AZ5214E resist