Specific Process Knowledge/Etch/III-V ICP/InP-InGaAsP-InGaAs: Difference between revisions
No edit summary |
|||
| Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Etch/III-V_ICP/InP-InGaAsP-InGaAs click here]''' | '''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Etch/III-V_ICP/InP-InGaAsP-InGaAs click here]''' | ||
== InP etch with HBr chemistry== | |||
Work done by Aurimas Sakanas @Fotonik.dtu 2019. This work was done to obtain very low surface roughness. | Work done by Aurimas Sakanas @Fotonik.dtu 2019. This work was done to obtain very low surface roughness. | ||
{| border="1" cellspacing="2" cellpadding="3" | {| border="1" cellspacing="2" cellpadding="3" | ||
| Line 68: | Line 68: | ||
</gallery> | </gallery> | ||
== InP etch with Cl2/H2 and a Si carrier wafer [[Image:section under construction.jpg|70px]] == | |||
''Work done by Berit Herstrøm @Nanolab spring 2019'' | ''Work done by Berit Herstrøm @Nanolab spring 2019'' | ||
{| border="1" cellspacing="2" cellpadding="3" | {| border="1" cellspacing="2" cellpadding="3" | ||
| Line 132: | Line 132: | ||
</gallery> | </gallery> | ||
== InP etch with Cl2/CH4/Ar 2013== | |||
Work done by Matthew Haines in 2013 <br> | Work done by Matthew Haines in 2013 <br> | ||
*[[Media:InP_Etch_Presentation_Final_Version-ky-bghe.pdf|InP Etch Presentation by Matthew Haines]] | *[[Media:InP_Etch_Presentation_Final_Version-ky-bghe.pdf|InP Etch Presentation by Matthew Haines]] | ||
== InP/InGaAsP/InGaAs etch 2011 == | |||
Unselective etch for large sized features and small aspect ratios by David Larsson, DTU Photonics, 2011 | Unselective etch for large sized features and small aspect ratios by David Larsson, DTU Photonics, 2011 | ||
Revision as of 14:21, 25 November 2019
Feedback to this page: click here
InP etch with HBr chemistry
Work done by Aurimas Sakanas @Fotonik.dtu 2019. This work was done to obtain very low surface roughness.
| Recipe name | ? |
| HBr flow | 10 sccm |
| CH4 flow | 5 sccm |
| Ar flow | 2 sccm |
| Platen power | 50 W |
| Coil power | 600 W |
| Pressure | 5 mTorr |
| Platen chiller temperature | 180 oC |
| Comment | Sample crystal bonded (Crystalbond 509, clear color) to Si carrier |
| Results | |
| Etch rate |
250-350 nm/min (2" wafer) |
| Sidewall angle |
85-87o (bottom) |
| Selectivity (InP:HSQ) | 15:1 (2"), 20:1 |
-
200 nm wide line structure, tetch=25 s
-
700 nm wide line structure, tetch=25 s
-
200 nm wide line structure, tetch=2 min
-
400 nm wide line structure, tetch=2 min
-
1 µm wide line structure, tetch=2 min
-
Two 1 µm wide line structure, 300 nm gap, tetch=25 s
-
Two 1 µm wide line structure, 300 nm gap, tetch=2 min
-
Two 1 µm wide line structure, 500 nm gap, tetch=2 min
-
Two 1 µm wide line structure, 1 µm gap, tetch=2 min
InP etch with Cl2/H2 and a Si carrier wafer 
Work done by Berit Herstrøm @Nanolab spring 2019
| Recipe name | ? |
| Cl2 flow | 6.6 sccm |
| H2 flow | 5.4 sccm |
| Process time | 6 min |
| Platen power | 150 W |
| Coil power | 800 W |
| Pressure | 0.5 mTorr (strike pressure 10s@10mTorr) |
| Platen chiller temperature | 180 oC |
| Comment | Sample placed on a Si carrier |
| Results | |
| Etch rate |
925 nm/min (small piece) |
| Sidewall angle |
90o (on this sample)
|
| Selectivity (InP:SiO2 (PECVD 500nm) | approx.17:1 |
| Other tests made | Comparing of this Cl2/H2 recipe with HBr recipe on e-beamed structures:Media:HBr vs Cl2 InP etch comparison Aurimas.pptx (By Aurimas Sakana @photonic (nov 2019))
|
InP etch with Cl2/CH4/Ar 2013
Work done by Matthew Haines in 2013
InP/InGaAsP/InGaAs etch 2011
Unselective etch for large sized features and small aspect ratios by David Larsson, DTU Photonics, 2011
| Recipe | InP Etch 1/InP Precond 1 |
| Cl2 flow | 20 sccm |
| N2 flow | 40 sccm |
| Ar flow | 10 sccm |
| Platen power | 100 W |
| Coil power | 500 W |
| Pressure | 2 mTorr |
| Platen chiller temperature | 180 oC |
| Comment | Use SiO2 carrier (not Si) (Kabi/Bghe June 2018) |
| Results (InP Etch 1) | |
| Etch rate | 500-600 nm/min |
| Sidewall angle | 86-87 o |
| Selectivity (InP:SiO2, InP:HSQ) | 50:1 |
- Result of InP etching. David Larsson, DTU Photonics, 2011
InP etching June 2018
Done by Kabi and Bghe @danchip
Sample pattern before etching
- Oxide mask before etching.
-
Top view of the SiO2 mask before etching
-
Top view of the SiO2 mask before etching
Etching of an InP piece on Si carrier
InP piece patterned with SiO2. The piece was etched on top of a Si wafer without bonding. The recipe "InP etch" was used. The roughness looks high in the bottom of the etched areas, especially in the large open areas.
- Result of InP etching.
-
low roughness in narrow trenched
-
low roughness in narrow trenched
-
A little higher roughnedd is larger trences
-
Much larger roughness in open areas
-
Zoom in on the large roughness
-
closed look at the large roughness in the open areas.
Etching of an InP piece on SiO2 carrier
InP piece patterned with SiO2. The piece was etched on top of a Si wafer coated with SiO2 without bonding. The recipe "InP etch" was used. The roughness looks low in the bottom of the etched areas, even in the large open areas.
- Result of InP etching.
-
Top view: oxide is gone on the narrow lines, low roughness in the trenches.
-
Top view: low roughness in the trenches.
-
30 dg view: low roughness in the trenches
-
30 dg view: low roughness in the trenches
-
Top view: low roughness in trench and in the large area
Changing the Cl2/N2 ratio
- Result of changing the Cl2/N2 ratio.
-
Sample S0: Top view of the oxide mask before etching. It is the TRAVKA50 mask, but it is clear that the CD reduction is about the 1-1.5 µm of the lines.
-
Sample S4: Profile view. The recipe InP etch has been used.
The sample has been run on a SiO2 carrier wafer.
There is not much CD change compared to the oxide mask before the etch.
It seems like the SiO2 mask is gone and the sidewall angle from the mask has been transferred into the sample.
The sidewall profile is quit vertical in the lower part.
Etch time 15 min
Etch depth in large open areas: 9.19µm -
Sample S5: Profile view. The recipe InP etch has been used but with modified Cl2 and N2 flows: N2=30 sccm Cl2=30 sccm.
The sample has been run on a SiO2 carrier wafer.
There is not much CD change compared to the oxide mask before the etch.
It seems like the SiO2 mask is gone.
The sidewall profile is overcutting probably due to too little passivation.
Etch time 10 min
Etch depth in large open areas: 11.82µm -
Sample S4: The sidewall roughness on the sample S4 is quit high
-
Sample S5: The sidewall roughness on the sample S5 is quit low.