An appropriate EBL resist must naturally be applied to the substrate. DTU Nanolab supplies a number of standard resists, please consult the table below. The default positive EBL resist is AR-P 6200.09 (CSAR). CSAR is installed on [[Specific_Process_Knowledge/Lithography/Coaters#Spin Coater: Gamma E-beam and UV|Spin Coater: Gamma E-beam and UV]] for spin coating of 2", 4" and 6" substrates. For other substrate sizes (i.e. chips) or other resists [[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|Spin Coater: LabSpin 02/03]] have to be used instead. The standard resist bottles are stored in the chemical cupboard in E-4. | An appropriate EBL resist must naturally be applied to the substrate. DTU Nanolab supplies a number of standard resists, please consult the table below. The default positive EBL resist is AR-P 6200.09 (CSAR). CSAR is installed on [[Specific_Process_Knowledge/Lithography/Coaters#Spin Coater: Gamma E-beam and UV|Spin Coater: Gamma E-beam and UV]] for spin coating of 2", 4" and 6" substrates. For other substrate sizes (i.e. chips) or other resists [[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|Spin Coater: LabSpin 02/03]] have to be used instead. The standard resist bottles are stored in the chemical cupboard in E-4. | ||
We recommend all groups or users to have their own bottle of e-beam resist inside the cleanroom. Please follow the [[Specific Process Knowledge/Lithography/EBeamLithography/ResistBottles|user resist bottles in the cleanroom guide.]] | We recommend all groups or users to have their own bottle of e-beam resist inside the cleanroom. Please follow the [[Specific Process Knowledge/Lithography/EBeamLithography/ResistBottles|user resist bottles in the cleanroom guide.]] | ||
==DTU Nanolab supplied EBL resists== | |||
<br> | |||
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" width="95%" | {|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" width="95%" | ||
|- | |- | ||
| Line 19: | Line 19: | ||
|'''Technical reports''' | |'''Technical reports''' | ||
|'''Spin Coater''' | |'''Spin Coater''' | ||
|'''Thinner''' | |'''Thinner''' | ||
|'''Developer''' | |'''Developer''' | ||
| Line 35: | Line 34: | ||
|[https://www.allresist.com/wp-content/uploads/sites/2/2020/03/AR-P6200_CSAR62english_Allresist_product-information.pdf AR-P 6200 info] | |[https://www.allresist.com/wp-content/uploads/sites/2/2020/03/AR-P6200_CSAR62english_Allresist_product-information.pdf AR-P 6200 info] | ||
|[[Specific_Process_Knowledge/Lithography/Coaters#Spin Coater: Gamma E-beam and UV|Spin Coater: Gamma E-beam and UV]] or [[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|Spin Coater: LabSpin 02/03]] | |[[Specific_Process_Knowledge/Lithography/Coaters#Spin Coater: Gamma E-beam and UV|Spin Coater: Gamma E-beam and UV]] or [[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|Spin Coater: LabSpin 02/03]] | ||
|Anisole | |Anisole | ||
| | | | ||
ZED N50 | |||
|IPA | |IPA | ||
| | | | ||
| Line 55: | Line 50: | ||
|[https://www.allresist.com/wp-content/uploads/sites/2/2020/03/SXAR-N8200-1_english_Allresist_product_information.pdf AR-N 8200 info] | |[https://www.allresist.com/wp-content/uploads/sites/2/2020/03/SXAR-N8200-1_english_Allresist_product_information.pdf AR-N 8200 info] | ||
|[[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|Spin Coater: LabSpin 02/03]] | |[[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|Spin Coater: LabSpin 02/03]] | ||
|AR 600-07 | |AR 600-07 | ||
|AR 300-47:DIW (1:1) | |AR 300-47:DIW (1:1) | ||
| Line 64: | Line 58: | ||
|- | |- | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
|'''[[ | |'''[[Specific Process Knowledge/Lithography/EBeamLithography/AR-N 7520 New|AR-N 7520 New]]''' | ||
|Negative | |Negative | ||
|[http://www.allresist.com AllResist] | |[http://www.allresist.com AllResist] | ||
|[ | |[[media:AR-N-7520New.pdf|AR-N7500New]] | ||
|[[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|Spin Coater: LabSpin 02/03]] | |[[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|Spin Coater: LabSpin 02/03]] | ||
|PGMEA | |PGMEA | ||
| | | | ||
*AR 300-47 | *AR 300-47 | ||
* | *MIF 726 | ||
| | |H2O | ||
| | | | ||
| | | | ||
| | |- | ||
|-style="background:LightGrey; color:black" | |||
|'''[[Specific Process Knowledge/Lithography/EBeamLithography/AR-P 617|AR-P 617]]''' | |||
|Positive | |||
|[http://www.allresist.com AllResist] | |||
|[https://www.allresist.com/wp-content/uploads/sites/2/2020/03/AR-P610_english_Allresist_product-information.pdf AR-P 617 info] | |||
|[[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|Spin Coater: LabSpin 02/03]] | |||
|PGMEA | |||
|AR 600-50 | |||
|IPA | |||
|Remover 1165 | |||
| | |||
Resist | |- | ||
|-style="background:WhiteSmoke; color:black" | |||
|'''[[Specific Process Knowledge/Lithography/EBeamLithography/ma-N 2400|ma-N 2400]]''' | |||
|Negative | |||
|[https://www.microresist.de/en/produkt/ma-n-2400-series/ Micro Resist Technology] | |||
| | |||
|[[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|Spin Coater: LabSpin 02/03]] | |||
|Anisole | |||
| | |||
*MIF 726 | |||
*ma-D 525 | |||
|H2O | |||
|mr-Rem 700 | |||
| | |||
|} | |||
<br> | |||
<br> | |||
==User supplied resists== | |||
It is possible to obtain permission to user other resists at DTU Nanolab, users must however provide these resists and possibly developers themselves. A non-exhaustive list of user supplied EBL resist used at DTU Nanolab and some process guidelines can be found in the table below. | It is possible to obtain permission to user other resists at DTU Nanolab, users must however provide these resists and possibly developers themselves. A non-exhaustive list of user supplied EBL resist used at DTU Nanolab and some process guidelines can be found in the table below. | ||
<br> | |||
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" width="95%" | {|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" width="95%" | ||
|- | |- | ||
| Line 127: | Line 145: | ||
|- | |- | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
|'''[[ | |'''[[Specific Process Knowledge/Lithography/EBeamLithography/AR-P 617|Copolymer AR-P 617]]''' | ||
|Positive | |Positive | ||
|[http://www.allresist.com AllResist] | |[http://www.allresist.com AllResist] | ||
| Line 141: | Line 159: | ||
|- | |- | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
|''' | |'''mr EBL 6000.1''' | ||
|Negative | |Negative | ||
|[http://http://www.microresist.de/home_en.htm MicroResist] | |[http://http://www.microresist.de/home_en.htm MicroResist] | ||
| Line 166: | Line 184: | ||
| | | | ||
|[[media:Process Flow HSQ.docx|process flow HSQ]] | |[[media:Process Flow HSQ.docx|process flow HSQ]] | ||
|- | |- | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
|'''AR-N | |'''AR-N 7500 <br> (not "New" Series)''' | ||
|Negative | |Negative | ||
|[http://www.allresist.com AllResist] | |[http://www.allresist.com AllResist] | ||
| | |[https://www.allresist.com/wp-content/uploads/sites/2/2020/03/AR-N7500_english_Allresist_product-information.pdf AR-N 7500] | ||
|[[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|Spin Coater: LabSpin 02/03]] | |||
| | |a = 17126, b = -0.435 | ||
|PGMEA | |PGMEA | ||
| | | | ||
*AR 300-47:DIW (4:1) | |||
*MIF726:DIW (8:5) | |||
|DIW | |||
| | |||
*AR 300-73 | |||
*O2 plasma | |||
| | | | ||
| Line 215: | Line 237: | ||
<br/> | <br/> | ||
==Current EBL resist stock== | |||
The table below indicates the current stock of Nanolab provided EBL resists in the resist cupboard in E4. | |||
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" width=" | {|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" width="800px" | ||
|- | |- | ||
| Line 229: | Line 252: | ||
|'''Expiration''' | |'''Expiration''' | ||
|'''Approximate amount remaining [L]''' | |'''Approximate amount remaining [L]''' | ||
|- | |||
|-style="background:LightGrey; color:black" | |||
|AR-P 6200.09 | |||
| 1 L | |||
| 2026 | |||
| 1 | |||
|- | |- | ||
| Line 260: | Line 290: | ||
|- | |- | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
|AR- | |AR-N 7520.11 New | ||
| 0.25 L | |||
| 2024 | |||
| 0.25 | |||
|- | |||
|-style="background:LightGrey; color:black" | |||
|AR-N 7520.17 New | |||
| 0.25 L | |||
| 2026 | |||
| 0.25 | |||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
|AR-N 7520.18 | |||
| 1 L | |||
| 2016 | |||
| 0.7 | |||
|- | |||
|-style="background:LightGrey; color:black" | |||
|AR-N 8200.06 | |||
| 0.1 L | | 0.1 L | ||
| 2021 | | 2021 | ||
| 0.1 | | 0.1 | ||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
|AR-N 8200.03 | |||
| 0.25 L | |||
| 2023 | |||
| 0.25 | |||
|} | |} | ||
=== Discharge layer application | <br clear="all" /> | ||
== Discharge layer application == | |||
As exposure is done with an electron beam, insulating substrates will cause a build up of charge that will deflect the incoming beam and disturb pattern definition. It is therefore necesarry when working with insulating substrates or substrates with thick (> 200 nm) dielectric films to apply a discharge layer. This is typically applied on top of the EBL resist layer and must be removed in between exposure and development. The most common discharge layer is 20 nm thermally evaporated Al. Bear in mind that it should be thermally evaporated and not e-beam evaporated. Thermal evaporation of Al can be done in [[Specific_Process_Knowledge/Thin film deposition/thermalevaporator|Thermal evaporator]] and [[Specific_Process_Knowledge/Thin film deposition/Wordentec|Wordentec]]. The Al layer can be removed with MIF726 after exposure. MIF726 etch rate in Al is about 0.5 nm/s, although only about 1 nm/min in oxidized aluminium. | As exposure is done with an electron beam, insulating substrates will cause a build up of charge that will deflect the incoming beam and disturb pattern definition. It is therefore necesarry when working with insulating substrates or substrates with thick (> 200 nm) dielectric films to apply a discharge layer. This is typically applied on top of the EBL resist layer and must be removed in between exposure and development. The most common discharge layer is 20 nm thermally evaporated Al. Bear in mind that it should be thermally evaporated and not e-beam evaporated. Thermal evaporation of Al can be done in [[Specific_Process_Knowledge/Thin film deposition/thermalevaporator|Thermal evaporator]] and [[Specific_Process_Knowledge/Thin film deposition/Wordentec|Wordentec]]. The Al layer can be removed with MIF726 after exposure. MIF726 etch rate in Al is about 0.5 nm/s, although only about 1 nm/min in oxidized aluminium. | ||
For samples with 2D materials such as graphene, HBN, etc., it is '''mandatory''' to apply a 20 nm Al layer on top of the resist in order to expose the substrate in the JEOL 9500 system. The Raith eLine system does not have this requirement. | For samples with 2D materials such as graphene, HBN, etc., it is '''mandatory''' to apply a 20 nm Al layer on top of the resist in order to expose the substrate in the JEOL 9500 system. The Raith eLine system does not have this requirement. | ||
== Inspection == | |||
Post exposure pattern dimensions are dependent on resist thickness. Thus, it is advisable to verify resist thickness after spin coating. This can be done by ellipsometry in the [[Specific_Process_Knowledge/Characterization/Optical_characterization#Ellipsometer|VASE Ellipsometer]]. | Post exposure pattern dimensions are dependent on resist thickness. Thus, it is advisable to verify resist thickness after spin coating. This can be done by ellipsometry in the [[Specific_Process_Knowledge/Characterization/Optical_characterization#Ellipsometer|VASE Ellipsometer]]. | ||