Jump to content

Specific Process Knowledge/Lithography/EBeamLithography/EBLsubstratePrep: Difference between revisions

Thope (talk | contribs)
Created page with "=== Resist coating === An appropriate EBL resist must naturally be applied to the substrate. DTU Nanolab supplies a number of standard resists, please consult the table below. The default positive EBL resist is AR-P 6200.09 (CSAR). CSAR installed on Spin Coater: Gamma E-beam and UV for spin coating of 2", 4" and 6" substrates. For other substrate sizes (i.e. chips) or other resists Spec..."
 
Elelop (talk | contribs)
No edit summary
 
(74 intermediate revisions by 3 users not shown)
Line 1: Line 1:
=== Resist coating ===
= Resist coating =
An appropriate EBL resist must naturally be applied to the substrate. DTU Nanolab supplies a number of standard resists, please consult the table below. The default positive EBL resist is AR-P 6200.09 (CSAR). CSAR installed on [[Specific_Process_Knowledge/Lithography/Coaters#Spin Coater: Gamma E-beam and UV|Spin Coater: Gamma E-beam and UV]] for spin coating of 2", 4" and 6" substrates. For other substrate sizes (i.e. chips) or other resists [[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|Spin Coater: LabSpin 02/03]] have to be used instead. The standard resist bottles are stored in the chemical cupboard in E-4.
An appropriate EBL resist must naturally be applied to the substrate. DTU Nanolab supplies a number of standard resists, please consult the table below. The default positive EBL resist is AR-P 6200.09 (CSAR). CSAR is installed on [[Specific_Process_Knowledge/Lithography/Coaters#Spin Coater: Gamma E-beam and UV|Spin Coater: Gamma E-beam and UV]] for spin coating of 2", 4" and 6" substrates. For other substrate sizes (i.e. chips) or other resists [[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|Spin Coater: LabSpin 02/03]] have to be used instead. The standard resist bottles are stored in the chemical cupboard in E-4.
 
 
Contrary to most UV resist it is in general not advisable to use HMDS priming when coating with EBL resists. There can of course be exceptions to this but we do not recommend HMDS priming when using the DTU Nanolab supplied EBL resists.
 


We recommend all groups or users to have their own bottle of e-beam resist inside the cleanroom. Please follow the [[Specific Process Knowledge/Lithography/EBeamLithography/ResistBottles|user resist bottles in the cleanroom guide.]]
We recommend all groups or users to have their own bottle of e-beam resist inside the cleanroom. Please follow the [[Specific Process Knowledge/Lithography/EBeamLithography/ResistBottles|user resist bottles in the cleanroom guide.]]


==DTU Nanolab supplied EBL resists==
<br>
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" width="95%"
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" width="95%"
|-
|-
Line 21: Line 19:
|'''Technical reports'''
|'''Technical reports'''
|'''Spin Coater'''
|'''Spin Coater'''
|'''Polynomial'''
|'''Thinner'''
|'''Thinner'''
|'''Developer'''
|'''Developer'''
Line 37: Line 34:
|[https://www.allresist.com/wp-content/uploads/sites/2/2020/03/AR-P6200_CSAR62english_Allresist_product-information.pdf AR-P 6200 info]  
|[https://www.allresist.com/wp-content/uploads/sites/2/2020/03/AR-P6200_CSAR62english_Allresist_product-information.pdf AR-P 6200 info]  
|[[Specific_Process_Knowledge/Lithography/Coaters#Spin Coater: Gamma E-beam and UV|Spin Coater: Gamma E-beam and UV]] or [[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|Spin Coater: LabSpin 02/03]]
|[[Specific_Process_Knowledge/Lithography/Coaters#Spin Coater: Gamma E-beam and UV|Spin Coater: Gamma E-beam and UV]] or [[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|Spin Coater: LabSpin 02/03]]
|a = 7252.2, b = -0.454
|Anisole
|Anisole
|
|
*AR-600-546
ZED N50
*AR-600-548
*N50  
*MIBK:IPA
|IPA
|IPA
|
|
Line 57: Line 50:
|[https://www.allresist.com/wp-content/uploads/sites/2/2020/03/SXAR-N8200-1_english_Allresist_product_information.pdf AR-N 8200 info]
|[https://www.allresist.com/wp-content/uploads/sites/2/2020/03/SXAR-N8200-1_english_Allresist_product_information.pdf AR-N 8200 info]
|[[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|Spin Coater: LabSpin 02/03]]
|[[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|Spin Coater: LabSpin 02/03]]
|a = ?, b = ?
|AR 600-07
|AR 600-07
|AR 300-47:DIW (1:1)
|AR 300-47:DIW (1:1)
Line 65: Line 57:


|-
|-
|-style="background:LightGrey; color:black"
|-style="background:WhiteSmoke; color:black"
|'''[[Specific_Process_Knowledge/Lithography/ARN7500|AR-N 7500]]'''
|'''[[Specific Process Knowledge/Lithography/EBeamLithography/AR-N 7520 New|AR-N 7520 New]]'''
|Negative
|Negative
|[http://www.allresist.com AllResist]
|[http://www.allresist.com AllResist]
|[https://www.allresist.com/wp-content/uploads/sites/2/2020/03/AR-N7500_english_Allresist_product-information.pdf AR-N 7500 info]
|[[media:AR-N-7520New.pdf‎|AR-N7500New]]
|[[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|Spin Coater: LabSpin 02/03]]
|[[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|Spin Coater: LabSpin 02/03]]
|a = 17126, b = -0.435
|PGMEA
|PGMEA
|
|
*AR 300-47:DIW (4:1)
*AR 300-47  
*MIF726:DIW (8:5)
*MIF 726
|DIW
|H2O
|
|
*AR 300-73
*O2 plasma
|
|


|}
|-
|-style="background:LightGrey; color:black"
|'''[[Specific Process Knowledge/Lithography/EBeamLithography/AR-P 617|AR-P 617]]'''
|Positive
|[http://www.allresist.com AllResist]
|[https://www.allresist.com/wp-content/uploads/sites/2/2020/03/AR-P610_english_Allresist_product-information.pdf AR-P 617 info]
|[[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|Spin Coater: LabSpin 02/03]]
|PGMEA
|AR 600-50
|IPA
|Remover 1165
|


Resist thickness as function of spin speed on Lab Spin 2/3 can be estimated from the parameters above as y = ax<sup>b</sup>, where y is resist thickness in nm and x is spin speed in RPM.
|-
|-style="background:WhiteSmoke; color:black"
|'''[[Specific Process Knowledge/Lithography/EBeamLithography/ma-N 2400|ma-N 2400]]'''
|Negative
|[https://www.microresist.de/en/produkt/ma-n-2400-series/ Micro Resist Technology]
|
|[[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|Spin Coater: LabSpin 02/03]]
|Anisole
|
*MIF 726
*ma-D 525
|H2O
|mr-Rem 700
|


|}
<br>
<br>


==User supplied resists==
It is possible to obtain permission to user other resists at DTU Nanolab, users must however provide these resists and possibly developers themselves. A non-exhaustive list of user supplied EBL resist used at DTU Nanolab and some process guidelines can be found in the table below.
It is possible to obtain permission to user other resists at DTU Nanolab, users must however provide these resists and possibly developers themselves. A non-exhaustive list of user supplied EBL resist used at DTU Nanolab and some process guidelines can be found in the table below.
 
<br>
 
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" width="95%"
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" width="95%"
|-
|-
Line 129: Line 145:
|-
|-
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
|'''[[Specific_Process_Knowledge/Lithography/ARP617|Copolymer AR-P 617]]'''
|'''[[Specific Process Knowledge/Lithography/EBeamLithography/AR-P 617|Copolymer AR-P 617]]'''
|Positive
|Positive
|[http://www.allresist.com AllResist]
|[http://www.allresist.com AllResist]
Line 143: Line 159:
|-
|-
|-style="background:LightGrey; color:black"
|-style="background:LightGrey; color:black"
|'''[[Specific_Process_Knowledge/Lithography/mrEBL6000|mr EBL 6000.1]]'''
|'''mr EBL 6000.1'''
|Negative
|Negative
|[http://http://www.microresist.de/home_en.htm MicroResist]
|[http://http://www.microresist.de/home_en.htm MicroResist]
Line 168: Line 184:
|
|
|[[media:Process Flow HSQ.docx|process flow HSQ]]
|[[media:Process Flow HSQ.docx|process flow HSQ]]
[[Specific_Process_Knowledge/Lithography/EBeamLithography/High_resolution_patterning_with_HSQ|High resolution patterning with HSQ]]
 


|-
|-
|-style="background:LightGrey; color:black"
|-style="background:LightGrey; color:black"
|'''AR-N 7520'''
|'''AR-N 7500 <br> (not "New" Series)'''
|Negative
|Negative
|[http://www.allresist.com AllResist]
|[http://www.allresist.com AllResist]
|Both e-beam, DUV and UV-sensitive resist. Currently being tested, contact [mailto:pxshi@dtu.dk Peixiong Shi] for information.
|[https://www.allresist.com/wp-content/uploads/sites/2/2020/03/AR-N7500_english_Allresist_product-information.pdf AR-N 7500]
|[[media:AR-N7500-7520.pdf‎|AR-N7500-7520]]
|[[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|Spin Coater: LabSpin 02/03]]
|See table <u>[[Specific_Process_Knowledge/Lithography/Coaters#Coaters:_Comparison_Table|here]] </u>
|a = 17126, b = -0.435
|PGMEA
|PGMEA
|AR 300-47, TMAH
|H2O
|
|
*AR 300-47:DIW (4:1)
*MIF726:DIW (8:5)
|DIW
|
*AR 300-73
*O2 plasma
|
|


Line 217: Line 237:
<br/>
<br/>


=== Discharge layer application ===
==Current EBL resist stock==
As exposure is done with an electron beam, insulating substrates will cause a build up of charge that will deflect the incoming beam and disturb pattern definition. It is therefore necesarry when working with insulating substrates or substrates with thick (> 200 nm) dielectric films to apply a discharge layer. This is typically applied on top of the EBL resist layer and must be removed in between exposure and development. The most common discharge layer is 20 nm thermally evaporated Al. Bear in mind that it should be thermally evaporated and not e-beam evaporated. Thermal evaporation of Al can be done in [[Specific_Process_Knowledge/Thin film deposition/thermalevaporator|Thermal evaporator]] and [[Specific_Process_Knowledge/Thin film deposition/Wordentec|Wordentec]]. The Al layer can be removed with MIF726 after exposure. MIF726 etch rate in Al is about 0.5 nm/s, although only about 1 nm/min in oxidized aluminium.
The table below indicates the current stock of Nanolab provided EBL resists in the resist cupboard in E4.
 
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" width="800px"
|-
 
!colspan="4" border="none" style="background:silver; color:black;" align="center"|Current EBL resist stock in E4 (updated 2023-09-04)
|-
 
|-
|-style="background:silver; color:black"
|'''Resist'''
|'''Bottle size'''
|'''Expiration'''
|'''Approximate amount remaining [L]'''
 
|-
|-style="background:LightGrey; color:black"
|AR-P 6200.09
| 1 L
| 2026
| 1
 
|-
|-style="background:WhiteSmoke; color:black"
|AR-P 6200.04
| 1 L
| 2026
| 1
 
|-
|-style="background:LightGrey; color:black"
|AR-P 6200.04
| 0.25 L
| 2019
| 0.25
 
|-
|-style="background:WhiteSmoke; color:black"
|AR-P 6200.04
| 0.25 L
| 2019
| 0.1
 
|-
|-style="background:LightGrey; color:black"
|AR-N 7520.07 New
| 1 L
| 2018
| 0.8
 
|-
|-style="background:WhiteSmoke; color:black"
|AR-N 7520.11 New
| 0.25 L
| 2024
| 0.25
 
|-
|-style="background:LightGrey; color:black"
|AR-N 7520.17 New
| 0.25 L
| 2026
| 0.25
 
|-
|-style="background:WhiteSmoke; color:black"
|AR-N 7520.18
| 1 L
| 2016
| 0.7
 
|-
|-style="background:LightGrey; color:black"
|AR-N 8200.06
| 0.1 L
| 2021
| 0.1
 
|-
|-style="background:WhiteSmoke; color:black"
|AR-N 8200.03
| 0.25 L
| 2023
| 0.25


For samples with 2D materials such as graphene, HBN, etc., it is '''mandatory''' to apply a 20 nm Al layer on top of the resist in order to expose the substrate in the JEOL 9500 system. The Raith eLine system does not have this requirement.
|}


Another possibility is to use a spin-on conductive layer such as [https://www.allresist.com/wp-content/uploads/sites/2/2021/05/Allresist_Product-information-Protective-Coating-AR-PC-5090_5091-English-web.pdf AR-PC 5090]. It can be removed with water after exposure. At the moment we do not have much experience with this, contact the EBL team if you are interested in this option.
<br clear="all" />


=== Inspection ===
== Discharge layer application ==
As exposure is done with an electron beam, insulating substrates will cause a build up of charge that will deflect the incoming beam and disturb pattern definition. It is therefore necesarry when working with insulating substrates or substrates with thick (> 200 nm) dielectric films to apply a discharge layer. This is typically applied on top of the EBL resist layer and must be removed in between exposure and development. The most common discharge layer is 20 nm thermally evaporated Al. Bear in mind that it should be thermally evaporated and not e-beam evaporated. Thermal evaporation of Al can be done in [[Specific_Process_Knowledge/Thin film deposition/thermalevaporator|Thermal evaporator]] and [[Specific_Process_Knowledge/Thin film deposition/Wordentec|Wordentec]]. The Al layer can be removed with MIF726 after exposure. MIF726 etch rate in Al is about 0.5 nm/s, although only about 1 nm/min in oxidized aluminium.


[[Image:RejectedSamples.png|500x500px|right|thumb|Example of rejected samples with visible bubbles in resist/Al coating and (a lot) of resist residue on the backside.]]
For samples with 2D materials such as graphene, HBN, etc., it is '''mandatory''' to apply a 20 nm Al layer on top of the resist in order to expose the substrate in the JEOL 9500 system. The Raith eLine system does not have this requirement.


== Inspection ==
Post exposure pattern dimensions are dependent on resist thickness. Thus, it is advisable to verify resist thickness after spin coating. This can be done by ellipsometry in the [[Specific_Process_Knowledge/Characterization/Optical_characterization#Ellipsometer|VASE Ellipsometer]].
Post exposure pattern dimensions are dependent on resist thickness. Thus, it is advisable to verify resist thickness after spin coating. This can be done by ellipsometry in the [[Specific_Process_Knowledge/Characterization/Optical_characterization#Ellipsometer|VASE Ellipsometer]].


Line 233: Line 338:


'''Samples with resist residues on the backside will also be rejected.''' If you have resist residues on the backside of your wafer you should wipe it off with an appropriate solvent.
'''Samples with resist residues on the backside will also be rejected.''' If you have resist residues on the backside of your wafer you should wipe it off with an appropriate solvent.
{| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;"
|-
| [[image:RejectedSamples.png|600px]]
|-
| colspan="1" style="text-align:center;|
Example of rejected samples with visible bubbles in resist/Al coating and (a lot) of resist residue on the backside. Photo: Thomas Pedersen.
|}


<br clear="all" />
<br clear="all" />