Jump to content

Specific Process Knowledge/Thin film deposition/PECVD: Difference between revisions

From LabAdviser
Jml (talk | contribs)
Bghe (talk | contribs)
 
(85 intermediate revisions by 7 users not shown)
Line 1: Line 1:
{{cc-nanolab}}
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/PECVD  click here]''' <br>
[[index.php?title=Category:Equipment|Thin film PECVD]]
[[index.php?title=Category:Thin Film Deposition|PECVD]]
==PECVD Plasma Enhanced Chemical Vapor Deposition==
==PECVD Plasma Enhanced Chemical Vapor Deposition==
[[image:Cluster1a.jpg|200x200px|right|thumb|PECVD1 (part of cluster1) - positioned in cleanroom2]]
Name PECVD4: PRO CVD <br>
[[image:PECVD3a.jpg|200x200px|right|thumb|PECVD3 - positioned in cleanroom1]]
Vendor: SPTS <br>
We have three PECVD's here at DANCHIP. They can all be used to deposit Silicon oxides and Silicon nitrides with or without dopants of Boron, Phosphorus and Germanium. PECVD1 and PECVD3 are used for silicon based processing where as PECVD2 is dedicated deposition on III-V materials. PECVD1 is the cleanest system where as PECVD3 is allowed to use with substrates with small abouts of metal on. See the precise rules in the equipment manuals which are uploaded in LabManager.
[[image:PECVD3a.jpg|300x300px|right|thumb|PECVD3 - positioned in cleanroom A-1, photo: DTU Nanolab internal]]
[[image:PECVD4.JPG|300x300px|right|thumb|PECVD4 - positioned in cleanroom B-1, photo: DTU Nanolab internal]]
We have two PECVD's here at DTU Nanolab. They can both be used to deposit Silicon oxides and Silicon nitrides with or without dopants of Boron and Phosphorus. PECVD3 can also deposit thin layer of aSi. PECVD3 is used for silicon based processing with small amounts (<5% wafer coverage, under some condition even more) of metals where as PECVD4 is dedicated for clean wafers both for silicon based materials and III-V materials. Quartz carriers are used in PECVD4 and they are dedicated the two different material groups to avoid cross contamination. See the precise rules in the equipment manuals which are uploaded in LabManager.


PECVD is a chemical vapor deposition process that applies a plasma to enhance chemical reaction rates of reactive spices. PECVD processing allows deposition at lower temperatures, which is often critical in the manufacture of semiconductors.
PECVD is a chemical vapor deposition process that applies a plasma to enhance chemical reaction rates of reactive species. PECVD processing allows deposition at lower temperatures, which is often critical in the manufacture of semiconductors. PECVD films are however known for not being stochiometeric and normally a lot of hydrogen is incorporated inside the films.


All though PECVD1, 2 and 3 are very similar you should not expect to transfer a recipe between the systems and get the same exact same result.
All though PECVD4 and 3 are very similar you should not expect to transfer a recipe between the systems and get the exact same result.


== Recipes on PECVD1 and PECVD3 ==
'''The user manuals, quality control procedures and results, user APVs, technical information and contact information can be found in LabManager (requires login):'''
*[[Specific Process Knowledge/Thin film deposition/Deposition of Silicon Oxide/Deposition of Silicon Oxide using PECVD#Recipes on PECVD1 for deposition of silicon oxides|Recipes on PECVD1 for deposition of silicon oxides]]
<!-- remember to remove the type of documents that are not present -->
*[[Specific Process Knowledge/Thin film deposition/Deposition of Silicon Nitride/Deposition of Silicon Nitride using PECVD#Recipes on PECVD1 for deposition of silicon nitride and silicon oxynitride|Recipes on PECVD1 for deposition of silicon nitride and silicon oxynitride]]
*[[Specific Process Knowledge/Thin film deposition/Deposition of Silicon Oxide/Deposition of Silicon Oxide using PECVD#Recipes on PECVD3 for deposition of silicon oxides|Recipes on PECVD3 for deposition of silicon oxides]]
*[[Specific Process Knowledge/Thin film deposition/Deposition of Silicon Nitride/Deposition of Silicon Nitride using PECVD#Recipes on PECVD3 for deposition of silicon nitride and silicon oxynitride|Recipes on PECVD3 for deposition of silicon nitride and silicon oxynitride]]
<br clear="all" />


<!-- give the link to the equipment info page in LabManager: -->
[http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=106  PECVD3 in LabManager]<br/>
[http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=395  PECVD4 in LabManager]
== Process information on PECVD3 and PECVD4==
*[[Specific Process Knowledge/Thin film deposition/Deposition of Silicon Oxide/Deposition of Silicon Oxide using PECVD|Recipes for deposition of silicon oxides]]
*[[Specific Process Knowledge/Thin film deposition/Deposition of Silicon Nitride/Deposition of Silicon Nitride using PECVD|Recipes on for deposition of silicon nitride and silicon oxynitride]]
*[[/Doping|Doping with boron]]
*[[/Pre-release tests on PECVD4|Pre-release tests on PECVD4]]
*[[Specific Process Knowledge/Thin film deposition/Deposition of Silicon/Si deposition using PECVD|Si deposition using PECVD3]]<br />
==Overview of the performance of PECVD thin films and some process related parameters==
==Overview of the performance of PECVD thin films and some process related parameters==


{| border="2" cellspacing="0" cellpadding="10"  
{| border="2" cellspacing="0" cellpadding="10"  
!colspan="2" border="none" style="background:silver; color:black;" align="center"|PECVD
|style="background:WhiteSmoke; color:black"|<b>PECVD3</b>
|style="background:WhiteSmoke; color:black"|<b>PECVD4</b>
|-
|-
!style="background:silver; color:black;" align="left"|Purpose  
!style="background:silver; color:black;" align="left"|Purpose  
Line 25: Line 45:
*Silicon nitride
*Silicon nitride
*Silicon oxynitride
*Silicon oxynitride
*PBSG (Phosphorous Boron doped Silica Glass)
*BPSG (Boron Phosphorous doped Silica Glass)
*Silicon oxide doped with Germanium
*aSi
|-
|
!style="background:silver; color:black" align="left"|Performance
|style="background:LightGrey; color:black"|Film thickness
|style="background:WhiteSmoke; color:black"|
*~10nm - 30µm
|-
|style="background:silver; color:black" |
|style="background:LightGrey; color:black"|Index of refraction
|style="background:WhiteSmoke; color:black"|
*~1.4-2.1
|-
|style="background:silver; color:black"|
|style="background:LightGrey; color:black"|Step coverage
|style="background:WhiteSmoke; color:black"|
*In general: Not so good
*PBSG: Floats at 1000<sup>o</sup>C
|-
|style="background:silver; color:black"|
|style="background:LightGrey; color:black"|Film quality
|style="background:WhiteSmoke; color:black"|
*Not so dense film
*Hydrogen will be incorporated in the films
|-
!style="background:silver; color:black" align="left"|Process parameter range
|style="background:LightGrey; color:black"|Process Temperature
|style="background:WhiteSmoke; color:black"|
*300 <sup>o</sup>C
|-
|style="background:silver; color:black"|
|style="background:LightGrey; color:black"|Process pressure
|style="background:WhiteSmoke; color:black"|
*~200-900 mTorr
|-
|style="background:silver; color:black"|
|style="background:LightGrey; color:black"|Gas flows
|style="background:WhiteSmoke; color:black"|
*SiH<math>_4</math>:0-60 sccm
*N<math>_2</math>O:0-3000 sccm
*NH<math>_3</math>:0-1000 sccm
*N<math>_2</math>:0-3000 sccm
*GeH<math>_4</math>:0-6.00 sccm
*5%PH<math>_3</math>:0-99 sccm
*5%B<math>_2</math>H<math>_6</math>:0-1000 sccm
|-
!style="background:silver; color:black" align="left"|Substrates
|style="background:LightGrey; color:black"|Batch size
|style="background:WhiteSmoke; color:black"|
*1-3 4" wafer per run
*1 6" wafer per run
*Or several smaler pieces
*Deposition on one side of the substrate
|-
|style="background:silver; color:black"|
| style="background:LightGrey; color:black"|Substrate material allowed
|style="background:WhiteSmoke; color:black"|
*Silicon wafers
**with layers of silicon oxide or silicon (oxy)nitride
*Quartz wafers
|-
|style="background:silver; color:black"|
| style="background:LightGrey; color:black"|Material allowed on the substrate
|style="background:WhiteSmoke; color:black"|
*Aluminium
*All metals < 5% of the substrate coverage (ONLY PECVD3!)
|-
|}
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
{| border="2" cellspacing="0" cellpadding="10"
|-
!style="background:silver; color:black;" align="left"|Purpose
|style="background:LightGrey; color:black"|Deposition of dielectrica
|style="background:WhiteSmoke; color:black"|
*Silicon oxide
*Silicon oxide
*Silicon nitride
*Silicon nitride
*Silicon oxynitride
*Silicon oxynitride
*PBSG (Phosphorous Boron doped Silica Glass)
*BPSG (Boron Phosphorous doped Silica Glass)
*Silicon oxide doped with Germanium
|-
|-
!style="background:silver; color:black" align="left" rowspan="4"|Performance
!style="background:silver; color:black" align="left" rowspan="4" valign="top" |Performance
|style="background:LightGrey; color:black"|Film thickness
|style="background:LightGrey; color:black"|Film thickness
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*~10nm - 30µm
*~10nm - 30µm (recipe dependant)
|
*~10nm - 30µm (recipe dependant)
|-
|-
|style="background:LightGrey; color:black"|Index of refraction
|style="background:LightGrey; color:black"|Index of refraction
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*~1.4-2.1
|
*~1.4-2.1
*~1.4-2.1
|-
|-
Line 133: Line 69:
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*In general: Not so good
*In general: Not so good
*PBSG: Floats at 1000<sup>o</sup>C
*BPSG: Floats at 1000<sup>o</sup>C
|
*In general: Not so good
*BPSG: Floats at 1000<sup>o</sup>C
|-
|-
|style="background:LightGrey; color:black"|Film quality
|style="background:LightGrey; color:black"|Film quality
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Not so dense film
*Hydrogen will be incorporated in the films
|
*Not so dense film
*Not so dense film
*Hydrogen will be incorporated in the films
*Hydrogen will be incorporated in the films
|-
|-
!style="background:silver; color:black" align="left" rowspan="3" |Process parameter range
!style="background:silver; color:black" align="left" rowspan="3"  valign="top" |Process parameter range
|style="background:LightGrey; color:black"|Process Temperature
|style="background:LightGrey; color:black"|Process Temperature
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*300 <sup>o</sup>C
|
*300 <sup>o</sup>C
*300 <sup>o</sup>C
|-
|-
|style="background:LightGrey; color:black"|Process pressure
|style="background:LightGrey; color:black"|Process pressure
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*~200-900 mTorr
|
*~200-900 mTorr
*~200-900 mTorr
|-
|-
|style="background:LightGrey; color:black"|Gas flows
|style="background:LightGrey; color:black"|Gas flows
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*SiH<math>_4</math>:0-60 sccm
*SiH<sub>4</sub>:0-180 sccm
*N<math>_2</math>O:0-3000 sccm
*N<sub>2</sub>O:0-3000 sccm
*NH<math>_3</math>:0-1000 sccm
*NH<sub>3</sub>:0-1000 sccm
*N<math>_2</math>:0-3000 sccm
*N<sub>2</sub>:0-3000 sccm
*GeH<math>_4</math>:0-6.00 sccm
*5%PH<sub>3</sub>:0-60 sccm
*5%PH<math>_3</math>:0-99 sccm
*3%B<sub>2</sub>H<sub>6</sub>:0-200 sccm
*5%B<math>_2</math>H<math>_6</math>:0-1000 sccm
|
*SiH<sub>4</sub>:0-60 sccm
*N<sub>2</sub>O:0-3000 sccm
*NH<sub>3</sub>:0-287 sccm
*N<sub>2</sub>:0-3000 sccm
*Ar:0-1415 sccm
*5%PH<sub>3</sub>:0-100 sccm
*3%B<sub>2</sub>H<sub>6</sub>:0-850 sccm
|-
|-
!style="background:silver; color:black" align="left" rowspan="3"|Substrates
!style="background:silver; color:black" align="left" rowspan="3" valign="top" |Substrates
|style="background:LightGrey; color:black"|Batch size
|style="background:LightGrey; color:black"|Batch size
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*1-3 4" wafer per run
*One 4" wafer per run
*1 6" wafer per run
*One 6" wafer per run
*Or several smaler pieces
*Or several smaller pieces on carrier wafer
*Deposition on one side of the substrate
|
*One to 7 2" wafer per run
*One 4" wafer per run
*One 6" wafer per run
*Or several smaller pieces
*Deposition on one side of the substrate
*Deposition on one side of the substrate
|-
|-
| style="background:LightGrey; color:black"|Substrate material allowed
| style="background:LightGrey; color:black"|Materials allowed
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Silicon wafers
*Silicon wafers, Quarts (fused silica) wafers
**with layers of silicon oxide or silicon (oxy)nitride
**Other material (can be allowed if less than 3.9 cm2 is exposed to the plasma (<5% coverage of a 4" wafer), please ask!
|
*Silicon wafers, Quartz (fused silica) wafers,
**with layers of silicon oxide or silicon (oxy)nitride
**with layers of silicon oxide or silicon (oxy)nitride
*Quartz wafers  
*III-V wafers (on special carriers)
|-
| style="background:LightGrey; color:black"|Material allowed on the substrate
|style="background:WhiteSmoke; color:black"|
*Aluminium
*All metals < 5% of the substrate coverage (ONLY PECVD3!)
|-  
|-  
|}
|}

Latest revision as of 11:32, 14 July 2026

The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.

Feedback to this page: click here

Thin film PECVD PECVD

PECVD Plasma Enhanced Chemical Vapor Deposition

Name PECVD4: PRO CVD
Vendor: SPTS

PECVD3 - positioned in cleanroom A-1, photo: DTU Nanolab internal
PECVD4 - positioned in cleanroom B-1, photo: DTU Nanolab internal

We have two PECVD's here at DTU Nanolab. They can both be used to deposit Silicon oxides and Silicon nitrides with or without dopants of Boron and Phosphorus. PECVD3 can also deposit thin layer of aSi. PECVD3 is used for silicon based processing with small amounts (<5% wafer coverage, under some condition even more) of metals where as PECVD4 is dedicated for clean wafers both for silicon based materials and III-V materials. Quartz carriers are used in PECVD4 and they are dedicated the two different material groups to avoid cross contamination. See the precise rules in the equipment manuals which are uploaded in LabManager.

PECVD is a chemical vapor deposition process that applies a plasma to enhance chemical reaction rates of reactive species. PECVD processing allows deposition at lower temperatures, which is often critical in the manufacture of semiconductors. PECVD films are however known for not being stochiometeric and normally a lot of hydrogen is incorporated inside the films.

All though PECVD4 and 3 are very similar you should not expect to transfer a recipe between the systems and get the exact same result.

The user manuals, quality control procedures and results, user APVs, technical information and contact information can be found in LabManager (requires login):

PECVD3 in LabManager
PECVD4 in LabManager

Process information on PECVD3 and PECVD4

Overview of the performance of PECVD thin films and some process related parameters

PECVD PECVD3 PECVD4
Purpose Deposition of dielectrica
  • Silicon oxide
  • Silicon nitride
  • Silicon oxynitride
  • BPSG (Boron Phosphorous doped Silica Glass)
  • aSi
  • Silicon oxide
  • Silicon nitride
  • Silicon oxynitride
  • BPSG (Boron Phosphorous doped Silica Glass)
Performance Film thickness
  • ~10nm - 30µm (recipe dependant)
  • ~10nm - 30µm (recipe dependant)
Index of refraction
  • ~1.4-2.1
  • ~1.4-2.1
Step coverage
  • In general: Not so good
  • BPSG: Floats at 1000oC
  • In general: Not so good
  • BPSG: Floats at 1000oC
Film quality
  • Not so dense film
  • Hydrogen will be incorporated in the films
  • Not so dense film
  • Hydrogen will be incorporated in the films
Process parameter range Process Temperature
  • 300 oC
  • 300 oC
Process pressure
  • ~200-900 mTorr
  • ~200-900 mTorr
Gas flows
  • SiH4:0-180 sccm
  • N2O:0-3000 sccm
  • NH3:0-1000 sccm
  • N2:0-3000 sccm
  • 5%PH3:0-60 sccm
  • 3%B2H6:0-200 sccm
  • SiH4:0-60 sccm
  • N2O:0-3000 sccm
  • NH3:0-287 sccm
  • N2:0-3000 sccm
  • Ar:0-1415 sccm
  • 5%PH3:0-100 sccm
  • 3%B2H6:0-850 sccm
Substrates Batch size
  • One 4" wafer per run
  • One 6" wafer per run
  • Or several smaller pieces on carrier wafer
  • Deposition on one side of the substrate
  • One to 7 2" wafer per run
  • One 4" wafer per run
  • One 6" wafer per run
  • Or several smaller pieces
  • Deposition on one side of the substrate
Materials allowed
  • Silicon wafers, Quarts (fused silica) wafers
    • with layers of silicon oxide or silicon (oxy)nitride
    • Other material (can be allowed if less than 3.9 cm2 is exposed to the plasma (<5% coverage of a 4" wafer), please ask!
  • Silicon wafers, Quartz (fused silica) wafers,
    • with layers of silicon oxide or silicon (oxy)nitride
  • III-V wafers (on special carriers)