| (287 intermediate revisions by 11 users not shown) |
| Line 1: |
Line 1: |
| = Strip Comparison Table = | | {{cc-nanolab}} |
| {| border="2" cellspacing="0" cellpadding="2"
| | |
| | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Lithography/Strip click here]''' |
| | |
| | [[Category: Equipment|Lithography strip]] |
| | [[Category: Lithography|Strip]] |
|
| |
|
| !colspan="2" border="none" style="background:silver; color:black;" align="center"|Equipment
| | __TOC__ |
| |style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Strip#Plasma Asher 1|Plasma Asher 1]]</b>
| |
| |style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Strip#Plasma Asher 1|Plasma Asher 1]]</b>
| |
| |style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Strip#III-V Plasma Asher|III-V Plasma Asher]]</b>
| |
| |style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Strip#Rough Acetone Strip|Rough Acetone Strip]]</b>
| |
| |style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Strip#Fine Acetone Strip|Fine Acetone Strip]]</b>
| |
|
| |
|
| | = Strip Comparison Table = |
| | {| class="wikitable" |
| |- | | |- |
| !style="background:silver; width:100px; color:black;" align="center"|Purpose | | ! |
| |style="background:LightGrey; color:black" | | ! [[Specific_Process_Knowledge/Lithography/Strip#Plasma Asher 3: Descum|Plasma Asher 3: Descum]] |
| |style="background:WhiteSmoke; color:black" | | ! [[Specific_Process_Knowledge/Lithography/Strip#Plasma_Asher_4|Plasma Asher 4 (Clean)]] |
| |All purposes | | ! [[Specific_Process_Knowledge/Lithography/Strip#Plasma Asher 5|Plasma Asher 5 (Dirty)]] |
| |style="background:WhiteSmoke; color:black" | | ! [[Specific_Process_Knowledge/Lithography/Strip#Resist Strip|Resist strip]] |
| |Clean wafers only, no metal | | ! [[Specific Process Knowledge/Lithography/LiftOff|Lift-off]] |
| |style="background:WhiteSmoke; color:black"
| | |- |
| |III-V materials only | | ! scope=row style="text-align: left;" | Purpose |
| | | Resist descum |
| | | | | |
| | *Resist stripping |
| | *Resist descum |
| | | | | |
| | | *Resist stripping |
| | *Resist descum |
| | | Resist stripping |
| | | Metal lift-off |
| | |- |
| | ! scope=row style="text-align: left;" | Method |
| | | Plasma ashing |
| | | Plasma ashing |
| | | Plasma ashing |
| | | Solvent & ultrasonication |
| | | Solvent & ultrasonication |
| |- | | |- |
| !style="background:silver; color:black" align="center" valign="center" rowspan="3"|Performance | | ! scope=row style="text-align: left;" | Process gasses |
| |style="background:LightGrey; color:black"|Minimum feature size
| | | O<sub>2</sub> (50 sccm) |
| |style="background:WhiteSmoke; color:black"| | |
| *
| |
| |style="background:WhiteSmoke; color:black"|
| |
| *
| |
| |style="background:WhiteSmoke; color:black"|
| |
| | | | | |
| | *O<sub>2</sub> (0-500 sccm) |
| | *N<sub>2</sub> (0-500 sccm) |
| | | | | |
| | | *O<sub>2</sub> (0-500 sccm) |
| | *N<sub>2</sub> (0-500 sccm) |
| | *CF<sub>4</sub> (0-200 sccm) |
| | | NA |
| | | NA |
| | |- |
| | ! scope=row style="text-align: left;" | Process power |
| | | 10-100 W (10-100%) |
| | | 150-1000 W |
| | | 150-1000 W |
| | | NA |
| | | NA |
| |- | | |- |
| |style="background:LightGrey; color:black"|Exposure light/filters/spectrum
| | ! scope=row style="text-align: left;" | Process solvent |
| |style="background:WhiteSmoke; color:black"| | | | NA |
| *
| | | NA |
| |style="background:WhiteSmoke; color:black"|
| | | NA |
| *
| | | |
| |style="background:WhiteSmoke; color:black"|
| | *NMP (Remover 1165) |
| * | | *IPA (rinsing agent) |
| |style="background:WhiteSmoke; color:black"|
| |
| * | |
| | | | | |
| | | *NMP (Remover 1165) |
| | *IPA (rinsing agent) |
| |- | | |- |
| |style="background:LightGrey; color:black"|Exposure mode
| | ! scope=row style="text-align: left;" | Substrate batch |
| |style="background:WhiteSmoke; color:black"|
| |
| *
| |
| |style="background:WhiteSmoke; color:black"|
| |
| *
| |
| |style="background:WhiteSmoke; color:black"|
| |
| *
| |
| |style="background:WhiteSmoke; color:black"|
| |
| *
| |
| | | | | |
| | | *Chips: several |
| | *50 mm wafer: several |
| | *100 mm wafer: 1 |
| | | |
| | *Chips: several |
| | *50 mm wafer: several |
| | *100 mm wafer: 1-25 |
| | *150 mm wafer: 1-25 |
| | *200 mm wafer: 1-25 |
| | | |
| | *Chips: several |
| | *50 mm wafer: several |
| | *100 mm wafer: 1-25 |
| | *150 mm wafer: 1-25 |
| | *200 mm wafer: 1-25 |
| | | |
| | *100 mm wafer: 1-25 |
| | *150 mm wafer: 1-25 |
| | | |
| | *100 mm wafer: 1-25 |
| | *150 mm wafer: 1-25 |
| |- | | |- |
| !style="background:silver; color:black" align="center" valign="center" rowspan="2"|Process parameter range | | ! scope=row style="text-align: left;" | Substrate materials |
| |style="background:LightGrey; color:black"|Positive Process
| | | |
| |style="background:WhiteSmoke; color:black"|
| | *<span style="color:red">'''No polymer substrates'''</span><br> |
| * | | *Silicon substrates |
| |style="background:WhiteSmoke; color:black"|
| | *III-V substrates |
| * | | *Glass substrates |
| |style="background:WhiteSmoke; color:black"|
| | *Films, or patterned films, of any material except type IV (Pb, Te) |
| * | |
| |style="background:WhiteSmoke; color:black"|
| |
| * | |
| | | | | |
| | | *<span style="color:red">'''No metals'''</span><br> |
| |-
| | *<span style="color:red">'''No metal oxides'''</span><br> |
| |style="background:LightGrey; color:black"|Negative Process
| | *<span style="color:red">'''No III-V materials'''</span><br> |
| |style="background:WhiteSmoke; color:black"|
| | *Silicon substrates |
| * | | *Glass substrates |
| |style="background:WhiteSmoke; color:black"|
| | *Polymer substrates |
| * | | *Films, or patterned films, of resists/polymers |
| |style="background:WhiteSmoke; color:black"|
| |
| * | |
| |style="background:WhiteSmoke; color:black"|
| |
| * | |
| | | | | |
| | | *Silicon substrates |
| |-
| | *III-V substrates |
| !style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
| | *Glass substrates |
| |style="background:LightGrey; color:black"|Batch size
| | *Polymer substrates |
| |style="background:WhiteSmoke; color:black"|
| | *Films, or patterned films, of any material except type IV (Pb, Te) |
| *<nowiki>1</nowiki> small samples | |
| *<nowiki>1</nowiki> 50 mm wafers | |
| *<nowiki>1</nowiki> 100 mm wafers
| |
| *<nowiki>1</nowiki> 150 mm wafers
| |
| |style="background:WhiteSmoke; color:black"|
| |
| *<nowiki>1</nowiki> 50 mm wafers
| |
| *<nowiki>1</nowiki> 100 mm wafers
| |
| *<nowiki>25</nowiki> 150 mm wafers with automatic handling
| |
| |style="background:WhiteSmoke; color:black"|
| |
| *<nowiki>1</nowiki> small samples
| |
| *<nowiki>1</nowiki> 50 mm wafers
| |
| *<nowiki>1</nowiki> 100 mm wafers | |
| *<nowiki>1</nowiki> 150 mm wafers | |
| |style="background:WhiteSmoke; color:black"|
| |
| * | |
| | | | | |
| | | *<span style="color:red">'''No metals'''</span><br> |
| |-
| | *<span style="color:red">'''No metal oxides'''</span><br> |
| | style="background:LightGrey; color:black"|Allowed materials
| | *Silicon substrates |
| |style="background:WhiteSmoke; color:black"|
| | *III-V substrates |
| *Si and silicon oxide, silicon nitride
| | *Glass substrates |
| *Quartz, pyrex | | *Polymer substrates |
| |style="background:WhiteSmoke; color:black"|
| | *Films, or patterned films, of resists/polymers |
| *Si and silicon oxide, silicon nitride | |
| *Quartz, pyrex
| |
| |style="background:WhiteSmoke; color:black"|
| |
| *III-V compounds | |
| |style="background:WhiteSmoke; color:black"|
| |
| * | |
| | | | | |
| |-
| | *Silicon substrates |
| | *III-V substrates (only if clean) |
| | *Glass substrates |
| | *Films, or patterned films, of any material except type IV (Pb, Te) |
| |} | | |} |
|
| |
| <br clear="all" /> | | <br clear="all" /> |
|
| |
|
| =Plasma Asher 1 = | | = Plasma Ashing process parameters= |
| [[Image:plasmaasher2.JPG|322 × 324px|thumb|The PlasmaAsher1 is placed in Cleanroom 3.]]
| |
| | |
| The Plasma Asher1( 300 auto load model) can be used for the following process:
| |
| | |
| *Photoresist stripping
| |
| *Surface cleaning after storage
| |
| *Surface cleaning after processes using oil pump or diffusion pump vacuum
| |
| *Surface cleaning as part of photolithography after wet developing of lacquer structures prior to wet or plasma etching
| |
| *Stripping of photoresist layers after etching, including after being exposed to high temperatures as after implantation, ion etching, sputter etching, RIE
| |
| *Removal of organic passivating layers and masks
| |
| *Etching of glass and ceramic
| |
| *Etching of SiO<math>_2</math>, Si<math>_3</math>N<math>_4</math>, Si
| |
| *Removal of polyimide layers
| |
| | |
| The machine can be used for almost every materials, but if you have any doubt about your materials are compatible with the plasma process it is better to ask photolithography group at Danchip.
| |
| | |
|
| |
|
| ==Overview of typical processes==
| | {| class="wikitable" |
| | |
| {| border="2" cellspacing="0" cellpadding="4" align="left" | |
| !
| |
| ! Photoresist stripping
| |
| ! Surface treatment of plastic, ceramic and metal
| |
| ! Ashing of organic material
| |
| |-
| |
| |'''Process pressure'''
| |
| |0.8- 1.0mbar
| |
| |0.5- 1.0mbar
| |
| |0.8-1.5mbar
| |
| |- | | |- |
| |'''Process gases''' | | ! !! [[Specific_Process_Knowledge/Lithography/Strip#Plasma_Asher_4|Resist stripping]] !! [[Specific_Process_Knowledge/Lithography/Descum#Plasma_Asher_3:_Descum|Descum]] !! [[Specific_Process_Knowledge/Lithography/Descum#Plasma_Asher_4|Descum]] !! Surface treatment !! Other ashing of organic material |
| |O<sub>2</sub>, N<sub>2</sub>
| |
| |O<math>_2</math>, CF<math>_4</math>, N<math>_2</math> or their mixtures | |
| |O<sub>2</sub> | |
| |- | | |- |
| |'''Process power''' | | ! scope=row style="text-align: left;" | Tool |
| |600-1000W | | | Plasma asher 4 & 5 || Plasma asher 3: Descum || Plasma asher 4 & 5 || Plasma asher 4 & 5 || Plasma asher 4 & 5 |
| |150-300W | |
| |1000W or less for heat- sensitive materials | |
| |- | | |- |
| |'''Process time''' | | ! scope=row style="text-align: left;" | Process pressure |
| |5-60min, depending of photoresist thickness | | | 1.3 mbar || 0.8 mbar || 1.3 mbar || 0.5-1.5 mbar || 0.5-1.5 mbar |
| |a few seconds to a few minutes | |
| |Between 0.5 and 20 hours, depending on the material | |
| |- | | |- |
| |'''Batch size''' | | ! scope=row style="text-align: left;" | Process gasses |
| |1-10 wafers at a time | | | |
| |1 wafer at a time | | *O<sub>2</sub> (100 sccm) |
| |1 wafer at a time, use a container: Petri dish, evaporating dish weighing dish, beaker, etc. | | *N<sub>2</sub> (100 sccm) |
| | | |
| | *O<sub>2</sub> (45 sccm) |
| | | |
| | *O<sub>2</sub> (100 sccm) |
| | *N<sub>2</sub> (100 sccm) |
| | | |
| | *O<sub>2</sub> |
| | *N<sub>2</sub> |
| | *CF<sub>4</sub> |
| | | |
| | *O<sub>2</sub> |
| |- | | |- |
| |'''Size of substrate'''
| | ! scope=row style="text-align: left;" | Process power |
| |2"-6"
| | | 1000 W || 100 W || 200 W || 150-1000 W || 150-1000 W |
| |2"-6" | |
| |2"-6" | |
| |- | | |- |
| |'''Allowed materials''' | | ! scope=row style="text-align: left;" | Process time |
| |All | | | 20-90 minutes || 1-10 minutes || 5-15 minutes || Seconds to minutes || Many hours, material dependent |
| |All | |
| |All | |
| | |
| |- | | |- |
| | ! scope=row style="text-align: left;" | Substrate batch |
| | | 1-25 || 1-2 || 1-25 || 1-25 || 1-25 |
| |} | | |} |
|
| |
|
| <br clear="all" /> | | <br clear="all" /> |
|
| |
|
| | {{:Specific Process Knowledge/Lithography/Strip/plasmaAsher03}} |
|
| |
|
| | {{:Specific Process Knowledge/Lithography/Strip/plasmaAsher04}} |
|
| |
|
| | {{:Specific Process Knowledge/Lithography/Strip/plasmaAsher05}} |
|
| |
|
| A typical process time for stripping of 1.5 µm AZ5214e resist is 15-25 min and for stripping of 9.5 µm AZ4562 resist is 20-35 min with the process parameters: 210ml O<math>_2</math>/min or mixture of 210ml O<math>_2</math>/min and 70ml N<math>_2</math>/min, power 1000W.
| | {{:Specific Process Knowledge/Lithography/Strip/resistStrip}} |
| | |
| =Plasma Asher 2 =
| |
| [[Image:Plasma_Asher_6inch.jpg|300x300px|thumb|Plasma asher for removing AZ resist on 6" wafers: positioned in cleanroom ? (class 10 yellow room)]]
| |
| | |
| The Plasma Asher 2 is the same as Plasma Asher 1 but has another loading system which is more convenient for batch loading of 6inch substrates.
| |
| | |
| In this machine, only O2 and N2 gases are used for processes (in PlasmaAsher1, CF4 is used as well).
| |
| | |
| The typical process parameters when operating the equipment:
| |
| *Photeresist stripping
| |
| Pressure: 0.8 - 1.0 mbar
| |
| | |
| Gas: O2
| |
| | |
| Power: 600 - 1000 watts
| |
| | |
| Time: 5 -30 min., depending on photoresist type and thickness
| |
| | |
| A typical process time for stripping of 1.5 um AZ5214e resist is 25 min for 6 wafers load in a boat, recipe 1.
| |
| | |
| A Descum process in manuel mode:O2:70, N2:70, power:150W, time:10min Be sure to wait for cooling if the mashine has been used at 1000W right before.
| |
| At a load at 2 Fused silicawafers resist removed 0.01-01,5um
| |
| | |
| The other materials have not been tested yet.
| |
| | |
| =Rough Acetone Strip=
| |
| {| border="1" cellspacing="0" cellpadding="4" align="right"
| |
| |[[Image:Acetone_rough.jpg|150x150px|thumb|Acetone bath "rough" for removing most of the resist]]
| |
| |[[Image:Acetone_fine.jpg|150x150px|thumb|Acetone bath "fine" for removing the rest of the resist incl. ultrasound]]
| |
| |-
| |
| |}
| |
|
| |
|
| This acetone strip is only for wafers without metal and SU-8.
| | {{:Specific Process Knowledge/Lithography/Strip/wetBench06and07}} |
|
| |
|
| There are two acetone bath: one rough for stripping the most of the resist from the surface and one fine with a ultrasound for cleaning the resists remains.
| | =Decommisioned tools= |
| | <span style="color:red">Plasma asher 1 was decommissioned 2024-12-02.</span> |
|
| |
|
| | [[Specific Process Knowledge/Lithography/Strip/PlasmaAsher1|Information about decommissioned tool can be found here.]] |
|
| |
|
| '''Here are the main rules for acetone strip use:'''
| |
| *Place the wafers in a wafer holder and put them in the first bath for 2-5 min, this time is depending how much resist you have on the surface.
| |
| *After the rough strip place your wafers directly in the final bath, switch on for the ultra sound and strip them for 2-3 min.
| |
| *Rinse your wafers for 4-5 min. in running water after stripping .
| |
|
| |
|
| <br clear="all" /> | | <span style="color:red">Plasma asher 2 was decommissioned 2024-12-02.</span> |
|
| |
|
| =Lift-off wet bench=
| | [[Specific Process Knowledge/Lithography/Strip/PlasmaAsher2|Information about decommissioned tool can be found here.]] |
| [[Image:Acetone_lift-off.jpg|300x300px|thumb|Acetone lift-off: positioned in cleanroom 3]]
| |
| This bench is only for wafers with metal!
| |
| | |
| Here are the main rules for lift-off bench use:
| |
| *Place the wafers in a dedicated wafer holder.
| |
| *Put the holder in the acetone and start the ultrasound. The strip off time is depending of resist thickness.
| |
| *Rinse your wafers for 4-5 min. in running water after stripping.
| |
| | |
| Find more info about the lift-off process here: [[Specific Process Knowledge/Photolithography/AZ5214E standard resist - reverse process]]
| |
| <br clear="all" /> | | <br clear="all" /> |
|
| |
| =Overview of acetone benches=
| |
|
| |
| {| border="2" cellspacing="0" cellpadding="4" align="left"
| |
| !
| |
| ! Acetone strip
| |
| ! Lift-off
| |
| |-
| |
| |'''General description'''
| |
| |
| |
| wet stripping of resist
| |
| |
| |
| lift-off process
| |
| |-
| |
| |'''Chemical solution'''
| |
| |CH<sub>3</sub>COCH<sub>3</sub>
| |
| |CH<sub>3</sub>COCH<sub>3</sub>
| |
| |-
| |
| |'''Process temperature'''
| |
| |20 <sup>o</sup>C
| |
|
| |
| |20 <sup>o</sup>C
| |
|
| |
| |-
| |
|
| |
| |'''Batch size'''
| |
| |
| |
| 1-25 wafers at a time
| |
| |
| |
| 1-25 wafer at a time
| |
| |-
| |
| |'''Size of substrate'''
| |
| |
| |
| 4" wafers
| |
| |
| |
| 4" wafers
| |
| |-
| |
| |'''Allowed materials'''
| |
| |
| |
| *Silicon
| |
| *Silicon Oxide
| |
| *Silicon Nitride
| |
| *Silicon Oxynitride
| |
|
| |
| |
| |
| *All metals
| |
|
| |
| |-
| |
| |}
| |