'''Feedback to this section''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/SU-8 click here]'''
{{cc-nanolab}}


SU-8 is an epoxy based negative i-line photoresist  with a high contrast. More then 10:1 aspect ratio imaging with vertical sidewalls is one of the widely used properties of this resist. It also has high chemical, plasma and temperature resistance after curing which makes it well suited for permanent use applications.
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/SU-8 click here]'''


'''''Note:''' Since the SU-8 is epoxy-based the user is required to take the mandatory epoxy course "Personlig sikkerhed ved arbejde med epoxy". Registration to this course can be found on Portalen under: [http://portalen.dtu.dk/DTU_Generelt/AHR/Ansat/Kompetenceudvikling/Kurser/Arbejdsmiljoe.aspx Arbejdsmiljø kurser]
[[Category:Lithography|Resist]]
''
[[Category:Resist|SU-8]]


In Danchip the SU-8 2000 product line is widely used, where the '''SU-8 2005''' and '''SU-8 2075''' are supplied by Danchip. Other resit formulation can be used but has to be ordered by the user him/herself.
__TOC__


Process recommendations:
==Resist description==
* a standard process consist of spinning, soft bake, exposure, post-exposure bake and development. Please notice that the entire process must be done continuously, meaning that it is not recommendable to spin the resist and then wait until the next day before exposing.
SU-8 is an epoxy based negative i-line photoresist  with a high contrast. More than 10:1 aspect ratio imaging with vertical sidewalls is one of the widely used properties of this resist. It also has high chemical, plasma and temperature resistance after curing which makes it well suited for permanent use applications.
* exposure using radiation above 350 nm is recommended. [[Specific Process Knowledge/Lithography/UVExposure#Aligner-6inch|Aligner-6inch]] uses a long-pass filter which reduces the i-line and blocks shorter wavelengths, while [[Specific Process Knowledge/Lithography/UVExposure#KS Aligner|KS Aligner]] and [[Specific_Process_Knowledge/Lithography/UVExposure#Aligner:_MA6_-_2|Aligner: MA6-2]] both have i-line filters.
 
* Controlled soft and post-exposure bakes are recommended and must be optimized for the specific application, but baseline parameters which can be used as a starting point will be given.
<span style="color:red">'''Note:''' Since the SU-8 is epoxy-based, users are required to take the mandatory epoxy safety course "Personlig sikkerhed ved arbejde med epoxy". Registration to this course can be found on [https://www.inside.dtu.dk/en/medarbejder/hr-og-arbejdsmiljoe/kompetenceudvikling/kursusoversigt_overside/kursusoversigt/arbejdsmiljoe-og-beredskabskurser/epoxy-kursus?fs=1 DTU Inside]</span> - '''requires login'''
 
In the cleanroom the SU-8 2000 product line is widely used, where the '''SU-8 2005''', '''SU-8 2035''', and '''SU-8 2075''' are supplied by Nanolab.
 
Considering discontinuation of the SU-8 2000 series we need to move to another product.
Kayaku Advanced Materials, USA (KAM)v has following recommendation:
 
Current Product Target Coat Thickness Recommended Product 
 
SU-8 2010 or less ≤ 10 μm SU-8 3000 or SU-8 TF 6000 series 
 
SU-8 2010 through SU-8 2050 10 μm ≤ x ≤ 50 μm SU-8 3000 series 
 
SU-8 2075 or greater > 50 μm SU-8 XFT75 & SU-8 XFT100
 
After an internal conversation we have decided to try new followings products:
 
SU8 3005 instead of SU8 2005 [https://kayakuam.com/products/su-8-3000/ Product information]
 
SU8 3035 instead of SU8 2035 [https://kayakuam.com/products/su-8-3000/ Product information]
 
SU8 XFT75 instead of SU8 2075 [https://kayakuam.com/su8xft/ Product information]
 
And we will also try a new formulation SU8 3025. [https://kayakuam.com/products/su-8-3000/ Product information]
 
 
 
'''Process recommendations:'''
* A standard process consist of spinning, soft bake, exposure, post-exposure bake and development. Please notice that the entire process must be done continuously, meaning that it is not recommendable to spin the resist and then wait until the next day before exposing
* Exposure using radiation above 350 nm is recommended
* Controlled soft and post-exposure bakes are recommended and must be optimized for the specific application, but baseline parameters which can be used as a starting point will be given


You can also take a look at a Ph.D thesis on the topic that you can find in Process2Share: http://process2share.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Photolithography/SU8#Reports]
==Pretreatment==
==Pretreatment==
* To dehydrate the surface, bake in 250C oven at least 30 min, the longer the bake the better. Baking overnight is recommended.
* To dehydrate the surface, bake in 250C oven at least 30 min - the longer the bake, the better. Baking overnight is recommended
* Another dehydration step can be done in the HMDS oven using recipe 9. This does not expose the wafers to HMDS but instead makes a bakeout at reduced pressure
* Another dehydration step can be done in the HMDS oven using recipe 9. This does not expose the wafers to HMDS but instead makes a bake-out at reduced pressure


==Spinning==
==Spinning==
SU-8 resist is designed to produce low defect coatings over a very broad range of films thickness.  
SU-8 resist is designed to produce low defect coatings over a very broad range of films thickness. [[Specific Process Knowledge/Lithography/Coaters#Spin_Coater:_RCD8|Spin Coater: RCD8]] is dedicated to spin all SU-8 resist formulations.
 


[[Specific Process Knowledge/Lithography/Coaters#Spin_Coater:_RCD8|Spin Coater: RCD8]] is dedicated to spin all SU-8 resist formulations, but [[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|Spin Coater: Manual All Resist]] can also be used.
'''Safety rules:'''<br>
To keep the cleanroom safe and odor free during the spinning, please follow the following rules:
* Always use point exhaust above the place, where you handle the resist
* When you move the wafers to the dedicated hotplates, always carry them in a closed container


To keep clean room safe and odor free during the spinning please follow the following simple rules:
* Always use point exhaust above the place you handle the resist.
* To minimize fumes of resist keep the wafers with resist in the extract box prior the baking.
[[Image:KS_Spinner_extract_box.png|500x500px|thumb|Extract box for unbaked wafers.]]
* When you move the wafers to the dedicated hot plates always carry them in a close container.


The recommended coating condition:
'''Recommenced spin coating conditions:'''<br>
* Do manual syringe dispense for the thin resists or use a syringe dispense system for the thick resists.
* Dispense manually from bottle/syringe for the thin resists or use a syringe dispense system for the thick resists
* Do static dispense: approximately 1 ml of SU-8 per inch substrate diameter.
* Use static dispense; approximately 1 ml of SU-8 per inch of substrate diameter
* For SU-8 layers thicker then 100 um use two/step spin coating procedure:
* For SU-8 layers thicker than 100 um use two-step spin coating procedure:
** spread cycle 500rpm, 100rpm/s, 5 sec following by  
** 5 second spread cycle 500 rpm, acceleration 100 rpm/s, following by:
** thickness definition cycle with the final spin speed
** thickness definition cycle with the final spin speed
** layer uniformity of the thick films can be improved by using a rotation cover (Gyrset), but remember the speed limitation 3000rpm.
** layer uniformity of the thick films can be improved by using a rotation cover (Gyrset), but remember the speed limitation is then 3000 rpm
* For SU-8 layers thinner then 10um the spread cycle can be omitted to improve the uniformity of the films.
* For SU-8 layers thinner than 10 um the spread cycle can be omitted to improve the uniformity of the films


Here are the spinning curves for SU-8 2002 and SU-8 2005.
[[media:Spinning_curves.xls|Spinning curves for SU-8 2002 and 2005.]]


* A rotation cover (Gyrset) can be also used in case you will spin less than 1um resit
'''Spin curves:'''
** 3000rpm, 300rpm/s, 30sec with gyrset gives appx. 850nm with SU-8 2002 (the test done by Thomas Buss from Nanotech).
Please notice that we do not have a spin curves for new formulations yet, but as soon as we have available data based on our experiments from cleanroom we will publish it.
Spin curves for SU-8 2002 and SU-8 2005 (from the old KS Spinner):
[[File:SU8 spinCurves 2002 2005.png|640px|thumb|right|Spin curves for SU-8 2002 and SU-8 2005.]]
* A rotation cover (Gyrset) can be also used in case you need to spin less than 1 um resist film
** 3000 rpm, 300 rpm/s, 30 sec with gyrset gives approximately 850 nm film thickness, when using SU-8 2002
* Another way to get a thinner film is to dilute SU-8 2002 in cyclopentanone solution
** 120 nm film: dilute 25 ml SU-8 2002 in 80 ml cyclopentanone, spin at 7000 rpm
** 60-80 nm film: dilute 5 ml SU-8 2002 in 32 ml cyclopentanone, spin at 2000 - 7000 rpm
<br clear="all" />


* Another way to get a thinner layer is dilute SU-8 2002 in cyclopentanone solution (25ml SU-8 in 80ml cyclopentanone) gives 120nm layer with 7000rpm spinning (the test done by Irene Fernandez-Cuesta and Nimi Gopalakrishnan from Nanotech).
==Baking==
SU-8 baking can be divided in 2 steps:
#Soft bake step after spinning
#Post exposure bake after exposure


* To achieve a thickness between 80nm and 60nm dilute SU-8 2002 in cycopentanone in proportion 5ml SU-8 to 32 ml cyclopentanone. This test is done by Luca Pietrobon from Nanotech. See the spinning curves here. [[media:5ml_SU8_2002_in32ml_cycl.PNG|Diluted SU8 2002.]]


==Baking==
The goal of the soft bake step is to reduce the amount of solvent in the photoresist layer. The applied heat evaporates the solvent from the resist film. The soft bake step is be done on dedicated SU-8 hotplates, and is usually done in one or two steps with a 5-8 deg/min temperature ramp between the steps.<br>
SU-8 baking can be divided in 2 steps: soft bake step after spinning and post exposure bake after exposure.
The soft bake temperature is typically between 20°C and 110°C, and the soft bake time depends on the film thickness. After soft bake the resist should be firm to the touch (not sticky), in order to be used in the exposure tools.


The goal of the soft bake step is reducing the amount of solvent in the photoresist layer. The heat application leads to the solvent diffusion to the resist surface and its evaporation. The soft bake step can be done on SU-8 hotplates, marked Hotplates 1 and 2 in LabManager, and usually done in one or two steps with 5-8 deg/min temperature ramp between steps. The soft bake temperature typically is between 20 and 110 C and the soft bake time depends on the film thickness.
The goal of the post exposure bake is to increase the polymerization reaction (the cross-linking). The post exposure step can be done on the same hotplates as the soft bake step, with the temperature range between 20°C and 120°C, and with temperature ramping of 5-8 deg/min.


The goal of the post exposure bake is increasing the polymerization reaction even the polymerization can in principle take place at room temperature. The post exposure step can be done at the same hotplates, as the soft bake step, with the temperature range between 20 and 120C and with temperature ramping 5-8 deg/min.
'''NB:''' It is important to do the post exposure bake immediately after exposure, to limit photoinitiator diffusion into unexposed areas.
It is important to do the post exposure bake immediately after exposure to limit photoinitiator diffusion into non-exposed areas.


==Exposure==
==Exposure==
The exposure step is usually done in near UV-radiation at aligners system which blocks the wavelengths below the i-line (365nm wavelength). [[Specific Process Knowledge/Lithography/UVExposure#Aligner-6inch|Aligner-6inch]] uses a long-pass filter which reduces the i-line and blocks shorter wavelengths, while [[Specific Process Knowledge/Lithography/UVExposure#KS Aligner|KS Aligner]] and [[Specific_Process_Knowledge/Lithography/UVExposure#Aligner:_MA6_-_2|Aligner: MA6-2]] both have i-line filters.
Exposing SU-8 is done using light sources at 375 nm or lower. SU-8 is not (practically) sensitive to 405 nm light and above.


Duration of the UV-exposure depends of resist thickness, but notice that if the UV exposure becomes long then the heating at the interface with the mask can cause formation of hard skin at the surface of SU-8 so called T-topping phenomena. The the main rule is if the dose of the exposure exceeds 250-300 mJ/cm2 it is recommended to do a multiple exposure instead and have a waiting time between the steps to allow the resist cool down.
'''Exposure in mask aligner:'''<br>
Duration of the UV-exposure depends of resist thickness, and if the UV exposure becomes too long, the heating at the interface between the mask and resist can cause formation of "hard skin" at the surface of the SU-8; the so-called T-topping phenomena. The rule of thumb is, that if the exposure dose exceeds 250-300 mJ/cm<sup>2</sup>, it is recommended to do multiple exposures instead, with a waiting time of 15 - 20 s between the exposure steps, to allow the resist cool down.
 
'''Exposure in maskless aligner:'''<br>
The required dose at 365 nm (MLA1) is higher than the optimal dose for mask aligner, typically by a factor of approximately 1.4. For exposure at 375 nm (MLA2), the required dose is significantly higher than at 365 nm, by a factor of 5-10.


==Developing==
==Developing==
Developing of the SU-8 patterns is done in the [[http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Development#SU8-Developer|special developing station]] placed in cleanroom C-1 at Danchip. Under developing the substrates are immersed in Propylene Glycol Methyl Ether Acetate (PGMEA) first in a bath marked "First" and after in a bath marked "Final".
'''Development speed:'''
*Puddle development in mr DEV 600 (PGMEA): ~20 µm/min
*Immersion development in mr DEV 600 (PGMEA): ~20 µm/min
 
 
'''Puddle development:'''<br>
Puddle development can be done in the Spin coater: gamma ebeam & UV using one of the predefined development sequences. The development is a puddle development, and it requires that the substrate does not have any through holes - if the substrate has holes, you need to use immersion development instead.


The development time is dependent on the layer thickness.


After the development the substrate must be rinsed with Isopropyl Alcohol (IPA) on both side for 30 sec. White traces during rinsing indicate incomplete development of SU-8.
'''Immersion development:'''<br>
Immersion development can be done in the [[Specific_Process_Knowledge/Lithography/Development#SU8-Developer|Developer:_SU8_(Wet_Bench)]]:
#The development time is dependent on the layer thickness. Minimum development time in "First" bath is 1 min per 20 µm resist film thickness
#After development the substrate must be rinsed with IPA on both sides for ~30 sec. White traces during rinsing indicates incomplete development of SU-8
#Finally the substrates are dried in air in the drying bath or with a nitrogen gun


Finally the substrates are dried in air in the drying box or with a nitrogen gun.
==Phd. work on the topic==
==PhD dissertations==
PhD Thesis by Thomas Anhøj (February 2007) on process optimization of 40 µm thick SU-8 25 for lab-on-a-chip.
*[https://orbit.dtu.dk/en/publications/fabrication-of-high-aspect-ratio-su-8-structures-for-integrated-s Fabrication of high aspect ratio SU-8 structures for integrated spectrometers]
*[https://labmanager.dtu.dk/view_binary.php?class=MiscDocument&id=4&name=TAA_Defense_070420.pdf Slides from defence] - '''requires login'''

Latest revision as of 10:51, 26 August 2026

The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.

Feedback to this page: click here

Resist description

SU-8 is an epoxy based negative i-line photoresist with a high contrast. More than 10:1 aspect ratio imaging with vertical sidewalls is one of the widely used properties of this resist. It also has high chemical, plasma and temperature resistance after curing which makes it well suited for permanent use applications.

Note: Since the SU-8 is epoxy-based, users are required to take the mandatory epoxy safety course "Personlig sikkerhed ved arbejde med epoxy". Registration to this course can be found on DTU Inside - requires login

In the cleanroom the SU-8 2000 product line is widely used, where the SU-8 2005, SU-8 2035, and SU-8 2075 are supplied by Nanolab.

Considering discontinuation of the SU-8 2000 series we need to move to another product. Kayaku Advanced Materials, USA (KAM)v has following recommendation:

Current Product Target Coat Thickness Recommended Product

SU-8 2010 or less ≤ 10 μm SU-8 3000 or SU-8 TF 6000 series

SU-8 2010 through SU-8 2050 10 μm ≤ x ≤ 50 μm SU-8 3000 series

SU-8 2075 or greater > 50 μm SU-8 XFT75 & SU-8 XFT100

After an internal conversation we have decided to try new followings products:

SU8 3005 instead of SU8 2005 Product information

SU8 3035 instead of SU8 2035 Product information

SU8 XFT75 instead of SU8 2075 Product information

And we will also try a new formulation SU8 3025. Product information


Process recommendations:

  • A standard process consist of spinning, soft bake, exposure, post-exposure bake and development. Please notice that the entire process must be done continuously, meaning that it is not recommendable to spin the resist and then wait until the next day before exposing
  • Exposure using radiation above 350 nm is recommended
  • Controlled soft and post-exposure bakes are recommended and must be optimized for the specific application, but baseline parameters which can be used as a starting point will be given

Pretreatment

  • To dehydrate the surface, bake in 250C oven at least 30 min - the longer the bake, the better. Baking overnight is recommended
  • Another dehydration step can be done in the HMDS oven using recipe 9. This does not expose the wafers to HMDS but instead makes a bake-out at reduced pressure

Spinning

SU-8 resist is designed to produce low defect coatings over a very broad range of films thickness. Spin Coater: RCD8 is dedicated to spin all SU-8 resist formulations.


Safety rules:
To keep the cleanroom safe and odor free during the spinning, please follow the following rules:

  • Always use point exhaust above the place, where you handle the resist
  • When you move the wafers to the dedicated hotplates, always carry them in a closed container


Recommenced spin coating conditions:

  • Dispense manually from bottle/syringe for the thin resists or use a syringe dispense system for the thick resists
  • Use static dispense; approximately 1 ml of SU-8 per inch of substrate diameter
  • For SU-8 layers thicker than 100 um use two-step spin coating procedure:
    • 5 second spread cycle 500 rpm, acceleration 100 rpm/s, following by:
    • thickness definition cycle with the final spin speed
    • layer uniformity of the thick films can be improved by using a rotation cover (Gyrset), but remember the speed limitation is then 3000 rpm
  • For SU-8 layers thinner than 10 um the spread cycle can be omitted to improve the uniformity of the films


Spin curves: Please notice that we do not have a spin curves for new formulations yet, but as soon as we have available data based on our experiments from cleanroom we will publish it. Spin curves for SU-8 2002 and SU-8 2005 (from the old KS Spinner):

Spin curves for SU-8 2002 and SU-8 2005.
  • A rotation cover (Gyrset) can be also used in case you need to spin less than 1 um resist film
    • 3000 rpm, 300 rpm/s, 30 sec with gyrset gives approximately 850 nm film thickness, when using SU-8 2002
  • Another way to get a thinner film is to dilute SU-8 2002 in cyclopentanone solution
    • 120 nm film: dilute 25 ml SU-8 2002 in 80 ml cyclopentanone, spin at 7000 rpm
    • 60-80 nm film: dilute 5 ml SU-8 2002 in 32 ml cyclopentanone, spin at 2000 - 7000 rpm


Baking

SU-8 baking can be divided in 2 steps:

  1. Soft bake step after spinning
  2. Post exposure bake after exposure


The goal of the soft bake step is to reduce the amount of solvent in the photoresist layer. The applied heat evaporates the solvent from the resist film. The soft bake step is be done on dedicated SU-8 hotplates, and is usually done in one or two steps with a 5-8 deg/min temperature ramp between the steps.
The soft bake temperature is typically between 20°C and 110°C, and the soft bake time depends on the film thickness. After soft bake the resist should be firm to the touch (not sticky), in order to be used in the exposure tools.

The goal of the post exposure bake is to increase the polymerization reaction (the cross-linking). The post exposure step can be done on the same hotplates as the soft bake step, with the temperature range between 20°C and 120°C, and with temperature ramping of 5-8 deg/min.

NB: It is important to do the post exposure bake immediately after exposure, to limit photoinitiator diffusion into unexposed areas.

Exposure

Exposing SU-8 is done using light sources at 375 nm or lower. SU-8 is not (practically) sensitive to 405 nm light and above.

Exposure in mask aligner:
Duration of the UV-exposure depends of resist thickness, and if the UV exposure becomes too long, the heating at the interface between the mask and resist can cause formation of "hard skin" at the surface of the SU-8; the so-called T-topping phenomena. The rule of thumb is, that if the exposure dose exceeds 250-300 mJ/cm2, it is recommended to do multiple exposures instead, with a waiting time of 15 - 20 s between the exposure steps, to allow the resist cool down.

Exposure in maskless aligner:
The required dose at 365 nm (MLA1) is higher than the optimal dose for mask aligner, typically by a factor of approximately 1.4. For exposure at 375 nm (MLA2), the required dose is significantly higher than at 365 nm, by a factor of 5-10.

Developing

Development speed:

  • Puddle development in mr DEV 600 (PGMEA): ~20 µm/min
  • Immersion development in mr DEV 600 (PGMEA): ~20 µm/min


Puddle development:
Puddle development can be done in the Spin coater: gamma ebeam & UV using one of the predefined development sequences. The development is a puddle development, and it requires that the substrate does not have any through holes - if the substrate has holes, you need to use immersion development instead.


Immersion development:
Immersion development can be done in the Developer:_SU8_(Wet_Bench):

  1. The development time is dependent on the layer thickness. Minimum development time in "First" bath is 1 min per 20 µm resist film thickness
  2. After development the substrate must be rinsed with IPA on both sides for ~30 sec. White traces during rinsing indicates incomplete development of SU-8
  3. Finally the substrates are dried in air in the drying bath or with a nitrogen gun

Phd. work on the topic

PhD dissertations

PhD Thesis by Thomas Anhøj (February 2007) on process optimization of 40 µm thick SU-8 25 for lab-on-a-chip.