Jump to content

Specific Process Knowledge/Thin film deposition/Deposition of Silicon: Difference between revisions

From LabAdviser
Jmli (talk | contribs)
No edit summary
Reet (talk | contribs)
 
(37 intermediate revisions by 6 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Silicon&action=edit click here]'''  
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Silicon&action=edit click here]'''  


<i> Unless otherwise stated, this page is written by <b>DTU Nanolab internal</b></i>


PolySilicon can be deposited in several Danchip tools. It can be sputtered, e-beam evaporated or be deposited in the PolySilicon furnaces. In the chart below you can compare the different deposition methods:
PolySilicon can be deposited in several Nanolab tools. It can be sputtered, e-beam evaporated or be deposited in the PolySilicon furnaces. In the chart below you can compare the different deposition methods:




==Deposition of PolySilicon using LPCVD==
==Deposition of PolySilicon using LPCVD==
DTU Nanolab has two furnaces for the deposition of [[Specific Process Knowledge/Thin film deposition/Furnace LPCVD PolySilicon | PolySilicon using Low Chemical Vapour Deposition]] (LPCVD).


DTU Nanolab has two furnaces for deposition of LPCVD (Low Chemical Vapour Deposition) polysilicon: A 6" furnace (installed in 2011) for deposition of standard polySi, amorphous polySi and boron doped polySi on 100 mm or 150 mm wafers and a 4" furnace (installed in 1995) for deposition of standard polySi, amorphous polySi, boron- and phosphorous doped polySi on 100 mm wafers. In LabManager the two furnaces are named "Furnace: LPCVD Poly-Si (4") (B4)" and "Furnace: LPCVD Poly-Si (6") (E2)", respectively.  
We have a 6" furnace (installed in 2011) for the deposition of standard polySi, amorphous polySi and boron doped polySi on 100 mm or 150 mm wafers and a 4" furnace (installed in 1995) for the deposition of standard polySi, amorphous polySi, boron- and phosphorous doped polySi on 100 mm wafers.  


*[[Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_polysilicon/Deposition_of_polysilicon_using_LPCVD/Standard_recipes,_QC_limits_and_results_for_the_4%22_polysilicon_furnace|Deposition of polysilicon using the 4" polysilicon furnace]]
In LabManager the two furnaces are named "Furnace: LPCVD Poly-Si (4") (B4)" and "Furnace: LPCVD Poly-Si (6") (E2)", respectively.
*[[Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_polysilicon/Deposition_of_polysilicon_using_LPCVD/Standard_recipes,_QC_limits_and_results_for_the_6%22_polysilicon_furnace|Deposition of polysilicon using the 6" polysilicon furnace]]


*[[Specific Process Knowledge/Thin film deposition/Furnace LPCVD PolySilicon/Standard recipes, QC limits and results for the 4" polysilicon furnace|Deposition of PolySilicon using the 4" PolySilicon Furnace]]


==Deposition of Silicon using sputter deposition technique==
*[[Specific Process Knowledge/Thin film deposition/Furnace LPCVD PolySilicon/Standard recipes, QC limits and results for the 6" polysilicon furnace|Deposition of PolySilicon using the 6" PolySilicon Furnace]]


At Nanolab you can also deposit silicon the using Wordentec, the Lesker Sputter system or the IBE Ionfab300 sputter systems. One of the advantages here is that you can deposit on any material you like.  
==Deposition of Silicon using PECVD==
 
At Nanolab you can also deposit silicon the using PECVD. The deposition temperature is 300 °C.
 
* [[/Si deposition using PECVD|Si deposition using PECVD3]]


* [[Specific Process Knowledge/Etch/IBE&frasl;IBSD Ionfab 300/IBSD of Si|Si deposition in IBE&frasl;IBSD Ionfab300]]
==Deposition of Silicon using sputter deposition==


==Deposition of Silicon using PECVD==
At Nanolab we can sputter silicon with the Lesker Sputter systems (both the single chamber and dual chamber systems). One of the advantages of sputtering is that you can deposit on almost any material you like. In the cluster system you can heat the substrate up to 600 °C.
 
* [[Specific Process Knowledge/Thin film deposition/Deposition of Silicon/Si sputter in Sputter-System Lesker|Si sputter deposition in the  Sputter-System (Lesker)]] - ''includes information on surface roughness and stress''
* [[Specific Process Knowledge/Thin film deposition/Deposition of Silicon/Si sputter in Sputter-System Metal-Oxide(PC1)|Si sputter deposition in the  Sputter-System Metal-Oxide(PC1)]]
* [[Specific Process Knowledge/Thin film deposition/Deposition of Silicon/Si sputter in Sputter-System Metal-Oxide(PC3)|Si sputter deposition in the  Sputter-System Metal-Oxide(PC3)]]
 
It was previosly possible to sputter Si with our [[Specific Process Knowledge/Etch/IBE⁄IBSD Ionfab 300| IonFab 300]]. You can read about the deposition conditions and results from that [[Specific Process Knowledge/Etch/IBE⁄IBSD Ionfab 300/IBSD of Si|here]].
 
Some parameters for sputter deposition of Si in the now-decomissioned Wordentec[[Specific Process Knowledge/Thin film deposition/Si sputter in Wordentec| are found here]].


At Nanolab you can also deposit silicon the using PECVD. The deposition temperature is 300 <sup>o</sup>C.
==Deposition of Silicon using e-beam evaporation==
It is possible to e-beam evaporate silicon at Nanolab using the [[Specific Process Knowledge/Thin film deposition/10-pocket e-beam evaporator|E-beam evaporator (10-pockets)]], where the substrate can be heated up to 250 °C. As with sputtering you can deposit on almost any material. In e-beam evaporation the deposition is line-of-sight and will be suitable for lift-off. However for 8" wafers the system is not optimized for lift-off on the full diameter of the wafer.


* [[/Si deposition using PECVD|Si deposition using PECVD3]]
* [[Specific Process Knowledge/Thin film deposition/Deposition of Silicon/Si evaporation in E-beam evaporator Temescal-2|Si evaporation in E-beam evaporator (10-pockets)]]


==Comparison of the methods for deposition of Silicon==
==Comparison of the methods for deposition of Silicon==
Line 31: Line 46:
!  
!  
! 4" and 6" Furnace PolySi ([[Specific Process Knowledge/Thin film deposition/Furnace LPCVD PolySilicon|Furnace LPCVD PolySi]])
! 4" and 6" Furnace PolySi ([[Specific Process Knowledge/Thin film deposition/Furnace LPCVD PolySilicon|Furnace LPCVD PolySi]])
! Sputter ([[Specific Process Knowledge/Thin film deposition/Wordentec|Wordentec]])
! PECVD ([[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]])
! Sputter ([[Specific Process Knowledge/Etch/IBE&frasl;IBSD Ionfab 300|IBE/IBSD Ionfab 300]])
! Sputter ([[Specific Process Knowledge/Thin film deposition/Lesker|Lesker]])
! Sputter ([[Specific Process Knowledge/Thin film deposition/Lesker|Lesker]])
! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/III-V Dielectric evaporator|III-V Dielectric evaporator]])
! Sputter ([[Specific Process Knowledge/Thin film deposition/Cluster-based multi-chamber high vacuum sputtering deposition system|Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3)]])
! PECVD ([[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]])
! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/10-pocket e-beam evaporator|E-beam evaporator (10-pockets)]])
|-  
|-  
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
! General description
! General description


|LPCVD (low pressure chemical vapour deposition) of polysilicon
| LPCVD (low pressure chemical vapour deposition) of a-Si and poly-Si
 
| Plasma Enhanced Chemical Vapor Deposition of Si
| Sputter deposition of Si.
| Sputter deposition of Si.
| Ion beam sputter deposition of Si.
| Sputter deposition of Si.  
| Sputter deposition of Si.  
| E-beam evaporation of Si.
| E-beam evaporation of Si.
|Plasma Enhanced Chemical Vapor Deposition.
|-
|-


|-style="background:LightGrey; color:black"
|-style="background:LightGrey; color:black"
! Doping facility
! Doping facility
|Can be doped with boron or phosphorus during deposition
|Yes, B (boron) and P (phosphorus)
|Yes, B and P
|None
|None
|None
|None
|None
|None
|None
|Yes, B and P
|-
|-
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
! Pre-clean
! Pre-clean
|New wafers can go directly into the furnace. Processed wafers have to be RCA cleaned
|New wafers can go directly into the furnace. Processed wafers have to be RCA cleaned
|RF Ar clean
|&nbsp;
|None
|RF Ar clean available
|None
|None
|RF Ar clean
|&nbsp;
|&nbsp;
|-
|-
|-style="background:LightGrey; color:black"
|-style="background:LightGrey; color:black"
! Layer thickness
! Layer thickness
|~50Å to 2µm, if thicker layers are needed please ask the furnace team.
|~5 nm to 2 µm, if thicker layers are needed please ask the furnace team.
|10Å to about 3000Å
|few nm to ~ 600 nm
|No defined limits
|few nm to >200 nm
|
|few nm to ?
|10Å to 2500Å
|few nm to 600 nm
|few nm to ~500nm
|-
|-


Line 82: Line 89:
! Deposition rate
! Deposition rate
|
|
*undoped, boron doped:~100Å/min
*undoped, boron doped:~100 Å/min
*Phosphorous doped:~20Å/min
*Phosphorous doped:~20 Å/min
|
|~6 Å/s can probably be higher
In the order of 1 Å/s, but dependent on process parameters. See more [[Specific Process Knowledge/Thin film deposition/Si sputter in Wordentec|here.]]
 
| About 5 nm/min. See more [[Specific_Process_Knowledge/Etch/IBE⁄IBSD_Ionfab_300/IBSD_of_Si|here.]]
| Depends on process parameters, roughly 0.2-2 Å/s. See Process Log.
| Depends on process parameters, roughly 1 Å/s.
|Depends on process parameters, at least 0.3 Å/s, see conditions [[Specific_Process_Knowledge/Thin_film_deposition/Cluster-based_multi-chamber_high_vacuum_sputtering_deposition_system#Standard_recipe_performance|here]]
|1Å/s to 5Å/s (see below).
| 1 Å/s
|~6Å/s can probably be higher
|-
|-
|-style="background:LightGrey; color:black"
|-style="background:LightGrey; color:black"
! Process temperature
! Process temperature
|560 <sup>o</sup>C (amorph) and 620 <sup>o</sup>C (poly)
|560 °C (amorphous) and 620 °C (poly)
|?
|300 °C
|Platen: 5-60 <sup>o</sup>C
|room temperature
|Wafers can be heated to 100-200°C
|room temperature to 600 °C
|20-250 <sup>o</sup>C
|room temperature to 250 °C
|300 <sup>o</sup>C
|-
|-


Line 104: Line 109:
! Step coverage
! Step coverage
|Good
|Good
|.
|Not known
|
|Poor
|Medium
|Medium
|Medium
|Medium - may be possible to improve using HIPIMS
|no step coverage unless using tilt holder, in which case the step coverage can be very good and can be tuned.
|-
|-


Line 114: Line 118:
! Adhesion
! Adhesion
|Good for fused silica, silicon oxide, silicon nitride, silicon
|Good for fused silica, silicon oxide, silicon nitride, silicon
|.
|Not tested, but do not deposit on top of silicon
|Not tested
|&nbsp;
|&nbsp;
|&nbsp;
|&nbsp;
|&nbsp;
|Not tested, but do not deposit on top of silicon
|-
|-


Line 127: Line 130:
*1-25 wafes (6" furnace)
*1-25 wafes (6" furnace)
|
|
*24x 2" wafers or
* Several small samples
*6x 4" wafers or
* 1-2x 50 mm wafer
*6x 6" wafers
| 
* Several small samples mounted with capton tape
* 1x 50 mm wafer
* 1x 100 mm wafer
* 1x 100 mm wafer
* 1x 150 mm wafer
* 1x 150 mm wafer
* 1x 200 mm wafer
|
|
* Up to 1x6" wafers
* Up to 1x6" wafers
* smaller pieces
* smaller pieces
|
|
* 2"
*Up to 10x6" or 4" wafers
* chips
*many smaller pieces
|
|
* Several small samples
*Up to 4 x 6" wafer or
* 1-2x 50 mm wafer
*3x 8" wafers (ask for special holder)
* 1x 100 mm wafer
*Many smaller pieces
* 1x 150 mm wafer


|-style="background:LightGrey; color:black"
|-style="background:LightGrey; color:black"
Line 156: Line 153:
**  from the A, B and E stack furnaces  
**  from the A, B and E stack furnaces  
* Quartz/fused silica wafers (RCA cleaned)  
* Quartz/fused silica wafers (RCA cleaned)  
| 
* Silicon wafers
* Quartz wafers
* Pyrex wafers
|
|
*Same materials as on the allowed materials below
*See the cross contamination sheets.
|
|
* Silicon wafers
* Almost any that does not degas, see cross-contamination sheet
* Quartz wafers
* Pyrex wafers
|
|
* Silicon wafers
*Almost any that does not degas at your intended substrate temperature. See also cross-contamination sheets.
* Quartz wafers
* Pyrex wafers
|
|
See the cross contamination sheet for PECVD3
*Almost any that does not degas at your intended substrate temperature. See also cross-contamination sheet.


|-
|-
Line 177: Line 166:
! Allowed material  
! Allowed material  


| Only those above (under allowed substrates).
| *Only those above (under allowed substrates).
|
*See the cross contamination sheets
|     
|     
* Silicon oxide
*Almost any that does not degas, see the cross-contamination sheet
* Silicon (oxy)nitride
* Photoresist
* PMMA
* Mylar
* SU-8
* Metals
|
|
* Silicon, silicon oxides, silicon nitrides
*Almost any that does not degas, see the cross-contamination sheets
* Metals from the +list
* Metals from the -list
* Alloys from the above list
* Stainless steel
* Glass
* III-V materials
* Resists
* Polymers
* Capton tape
|   
* Silicon oxide
* Silicon (oxy)nitride
* Photoresist
* Metals
|     
* III-V materials
* Silicon wafers
* Resists
|
|
See the cross contamination sheet for PECVD3
*Almost any that does not degas, see cross-contamination sheet
 
|-
|-


Line 214: Line 182:
! Comment
! Comment
|
|
|Only in PECVD3
|  
|  
| The system is used both for IBSD and IBE. Si deposition can only be performed when it is set up for IBSD.
|
|  
|
| &nbsp;
|Only in PECVD3
|}
|}

Latest revision as of 00:22, 8 July 2025

Feedback to this page: click here

Unless otherwise stated, this page is written by DTU Nanolab internal

PolySilicon can be deposited in several Nanolab tools. It can be sputtered, e-beam evaporated or be deposited in the PolySilicon furnaces. In the chart below you can compare the different deposition methods:


Deposition of PolySilicon using LPCVD

DTU Nanolab has two furnaces for the deposition of PolySilicon using Low Chemical Vapour Deposition (LPCVD).

We have a 6" furnace (installed in 2011) for the deposition of standard polySi, amorphous polySi and boron doped polySi on 100 mm or 150 mm wafers and a 4" furnace (installed in 1995) for the deposition of standard polySi, amorphous polySi, boron- and phosphorous doped polySi on 100 mm wafers.

In LabManager the two furnaces are named "Furnace: LPCVD Poly-Si (4") (B4)" and "Furnace: LPCVD Poly-Si (6") (E2)", respectively.

Deposition of Silicon using PECVD

At Nanolab you can also deposit silicon the using PECVD. The deposition temperature is 300 °C.

Deposition of Silicon using sputter deposition

At Nanolab we can sputter silicon with the Lesker Sputter systems (both the single chamber and dual chamber systems). One of the advantages of sputtering is that you can deposit on almost any material you like. In the cluster system you can heat the substrate up to 600 °C.

It was previosly possible to sputter Si with our IonFab 300. You can read about the deposition conditions and results from that here.

Some parameters for sputter deposition of Si in the now-decomissioned Wordentec are found here.

Deposition of Silicon using e-beam evaporation

It is possible to e-beam evaporate silicon at Nanolab using the E-beam evaporator (10-pockets), where the substrate can be heated up to 250 °C. As with sputtering you can deposit on almost any material. In e-beam evaporation the deposition is line-of-sight and will be suitable for lift-off. However for 8" wafers the system is not optimized for lift-off on the full diameter of the wafer.

Comparison of the methods for deposition of Silicon

4" and 6" Furnace PolySi (Furnace LPCVD PolySi) PECVD (PECVD) Sputter (Lesker) Sputter (Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3)) E-beam evaporation (E-beam evaporator (10-pockets))
General description LPCVD (low pressure chemical vapour deposition) of a-Si and poly-Si Plasma Enhanced Chemical Vapor Deposition of Si Sputter deposition of Si. Sputter deposition of Si. E-beam evaporation of Si.
Doping facility Yes, B (boron) and P (phosphorus) Yes, B and P None None None
Pre-clean New wafers can go directly into the furnace. Processed wafers have to be RCA cleaned   None RF Ar clean available None
Layer thickness ~5 nm to 2 µm, if thicker layers are needed please ask the furnace team. few nm to ~ 600 nm few nm to >200 nm few nm to ? few nm to 600 nm
Deposition rate
  • undoped, boron doped:~100 Å/min
  • Phosphorous doped:~20 Å/min
~6 Å/s can probably be higher Depends on process parameters, roughly 0.2-2 Å/s. See Process Log. Depends on process parameters, at least 0.3 Å/s, see conditions here 1 Å/s
Process temperature 560 °C (amorphous) and 620 °C (poly) 300 °C room temperature room temperature to 600 °C room temperature to 250 °C
Step coverage Good Medium Medium Medium - may be possible to improve using HIPIMS no step coverage unless using tilt holder, in which case the step coverage can be very good and can be tuned.
Adhesion Good for fused silica, silicon oxide, silicon nitride, silicon Not tested, but do not deposit on top of silicon      
Batch size
  • 1-30 wafers (4" furnace)
  • 1-25 wafes (6" furnace)
  • Several small samples
  • 1-2x 50 mm wafer
  • 1x 100 mm wafer
  • 1x 150 mm wafer
  • Up to 1x6" wafers
  • smaller pieces
  • Up to 10x6" or 4" wafers
  • many smaller pieces
  • Up to 4 x 6" wafer or
  • 3x 8" wafers (ask for special holder)
  • Many smaller pieces
Allowed substrates
  • Silicon wafers (new or RCA cleaned)
    • with layers of silicon oxide or silicon (oxy)nitride
    • from the A, B and E stack furnaces
  • Quartz/fused silica wafers (RCA cleaned)
  • See the cross contamination sheets.
  • Almost any that does not degas, see cross-contamination sheet
  • Almost any that does not degas at your intended substrate temperature. See also cross-contamination sheets.
  • Almost any that does not degas at your intended substrate temperature. See also cross-contamination sheet.
Allowed material *Only those above (under allowed substrates).
  • See the cross contamination sheets
  • Almost any that does not degas, see the cross-contamination sheet
  • Almost any that does not degas, see the cross-contamination sheets
  • Almost any that does not degas, see cross-contamination sheet
Comment Only in PECVD3