Jump to content

Specific Process Knowledge/Lithography/Development: Difference between revisions

From LabAdviser
Lgpe (talk | contribs)
Jehem (talk | contribs)
 
(118 intermediate revisions by 7 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Development click here]'''
{{cc-nanolab}}


==Developement Comparison Table==
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Lithography/Development click here]'''


{| border="2" cellspacing="0" cellpadding="2"
[[Category: Equipment|Lithography development]]
[[Category: Lithography|Development]]
 
__TOC__


!colspan="2" border="none" style="background:silver; color:black;" align="center"|Equipment
==Development Comparison Table==
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Development#Developer-1 and Developer-2|Developer-1 and 2]]</b>
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Development#Developer-6inch|Developer: 6inch]]</b>
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Development#SU8-Developer|SU8-Developer]]</b>
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Development#Developer: E-beam Manual|Developer:E-beam Manual]]</b>
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Development#Developer:_TMAH_Manual|Developer: TMAH Manual]]</b>
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Development#Developer_TMAH_UV-lithography|Developer: TMAH UV-lithography]]</b>


{| class="wikitable"
|-
|-
!style="background:silver; color:black" align="center" width="60"|Purpose
!
|style="background:LightGrey; color:black"|
! [[Specific_Process_Knowledge/Lithography/Development#Manual_beaker_development_in_fumehood|Manual beaker development]]
|style="background:WhiteSmoke; color:black" align="center"|
! [[Specific_Process_Knowledge/Lithography/Development#Developer: SU8 (Wet Bench)|Developer: SU8 (Wet bench)]]
Development of
! [[Specific_Process_Knowledge/Lithography/Development#Developer: E-beam 02|Developer: E-beam 02]]
*AZ 5214E
! [[Specific_Process_Knowledge/Lithography/Development#Developer:_TMAH_Manual 02|Developer: TMAH Manual 02]]
*AZ 4562
! [[Specific_Process_Knowledge/Lithography/Development#Developer_TMAH_UV-lithography|Developer: TMAH UV-lithography]]
|style="background:WhiteSmoke; color:black" align="center"|
! [[Specific_Process_Knowledge/Lithography/Development/DUV_developer#Developer:_TMAH_Stepper|Developer: TMAH Stepper]]
Development of
|-
*AZ 5214E
! scope=row style="text-align: left;" | Purpose
*AZ 4562
|
|style="background:WhiteSmoke; color:black" align="center"|
Fall-back option if you have a process, which is not compatible with the automatic, or semi-automatic, tools
Development of
 
<span style="color:red">Requires individual risk assessment for TMAH development!</span>
|
Development of:
*SU-8
*SU-8
|style="background:WhiteSmoke; color:black" align="center"|
|
Development of
Development of:
*CSAR
*ZEP 520A
*Zep520A
*AR-P 6200.xx (CSAR)
|style="background:WhiteSmoke; color:black" align="center"|
|  
Development of
Development of:
*AZ nLOF
*AZ nLOF
*AZ MiR 701
*AZ MiR 701
Line 38: Line 39:
*AZ 4562
*AZ 4562
*DUV resists
*DUV resists
|style="background:WhiteSmoke; color:black" align="center"|
|  
Development of
Development of:
*AZ nLOF
*AZ nLOF
*AZ MiR 701
*AZ MiR 701
Line 46: Line 47:
*DUV resists
*DUV resists
Post-exposure baking
Post-exposure baking
 
|
Development of:
*DUV resists
Post-exposure baking
|-
|-
!style="background:silver; color:black" align="center" width="60"|Developer  
! scope=row style="text-align: left;" | Developer
|style="background:LightGrey; color:black"|
| Process dependent
|style="background:WhiteSmoke; color:black" align="center"|
| mr-Dev 600 (PGMEA)
AZ 351B diluted 1:5 in water
|  
 
*ZED N-50
(NaOH and sodium borate salt)
*AR 600-50
|style="background:WhiteSmoke; color:black" align="center"|
| AZ 726 MIF (2.38% TMAH in water)
AZ 351B diluted 1:5 in water
| AZ 726 MIF (2.38% TMAH in water)
 
| AZ 726 MIF (2.38% TMAH in water)
(NaOH and sodium borate salt)
|style="background:WhiteSmoke; color:black" align="center"|
mr-Dev 600
 
(PGMEA)
|style="background:WhiteSmoke; color:black" align="center"|
N-50
AR600-546
|style="background:WhiteSmoke; color:black" align="center"|
AZ 726 MIF
 
(2.38% TMAH in water)
|style="background:WhiteSmoke; color:black" align="center"|
AZ 726 MIF
 
(2.38% TMAH in water)
 
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Method
! scope=row style="text-align: left;" | Method
|style="background:LightGrey; color:black"|Development
| Submersion
|style="background:WhiteSmoke; color:black" align="center"|
| Submersion
Submersion
| Puddle
|style="background:WhiteSmoke; color:black" align="center"|
| Puddle
Submersion
| Puddle
|style="background:WhiteSmoke; color:black" align="center"|
| Puddle
Submersion
|style="background:WhiteSmoke; color:black" align="center"|
Spray/Puddle
|style="background:WhiteSmoke; color:black" align="center"|
Spray/Puddle
|style="background:WhiteSmoke; color:black" align="center"|
Puddle
|-
|-
|style="background:LightGrey; color:black"|Handling
! scope=row style="text-align: left;" | Handling
|style="background:WhiteSmoke; color:black" align="center"|
|
Cassette
Manual handling in beakers
|style="background:WhiteSmoke; color:black" align="center"|
*Chip bucket
Cassette
*Single wafer carrier
|style="background:WhiteSmoke; color:black" align="center"|
*Carrier for up to 5 wafers
Single wafer holder
|
|style="background:WhiteSmoke; color:black" align="center"|
*Chip bucket
Vacuum chuck for 2",4" and 6" (the same) or chip "basket"
*Single wafer carrier
|style="background:WhiteSmoke; color:black" align="center"|
*Carrier for up to 6 wafers
Edge handling chuck or chip "basket"
|
|style="background:WhiteSmoke; color:black" align="center"|
*Vacuum-free edge-grip chucks for 50 mm, 100 mm & 150 mm, and 200 mm substrates
Vacuum chuck
*Chip chuck for chips & 2" substrates
|
*Vacuum-free edge-grip chucks for 50 mm, 100 mm & 150 mm, and 200 mm substrates
*Chip chuck for chips & 2" substrates
| Vacuum chuck
| Vacuum chuck
|-
|-
 
! scope=row style="text-align: left;" | Process temperature
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Process parameters
| Room temperature
|style="background:LightGrey; color:black"|Temperature
| Room temperature
|style="background:WhiteSmoke; color:black" align="center"|
| Room temperature
22°C
| Room temperature
|style="background:WhiteSmoke; color:black" align="center"|
| Room temperature
22°C
| Room temperature
|style="background:WhiteSmoke; color:black" align="center"|
Room temperature
|style="background:WhiteSmoke; color:black" align="center"|
Room temperature
|style="background:WhiteSmoke; color:black" align="center"|
Room temperature
|style="background:WhiteSmoke; color:black" align="center"|
Room temperature
|-
|-
|style="background:LightGrey; color:black"|Agitation
! scope=row style="text-align: left;" | Process agitation
|style="background:WhiteSmoke; color:black" align="center"|
| No agitation allowed
Manual
| Magnetic stirrer
|style="background:WhiteSmoke; color:black" align="center"|
| Rotation
Circulation and mechanical
| Rotation
|style="background:WhiteSmoke; color:black" align="center"|
| Rotation
Magnetic stirrer
| Rotation
|style="background:WhiteSmoke; color:black" align="center"|
Rotation
|style="background:WhiteSmoke; color:black" align="center"|
Rotation
|style="background:WhiteSmoke; color:black" align="center"|
Rotation
|-
|-
|style="background:LightGrey; color:black"|Rinse
! scope=row style="text-align: left;" | Process rinse
|style="background:WhiteSmoke; color:black" align="center"|
| Process dependent
DI water
| IPA
|style="background:WhiteSmoke; color:black" align="center"|
| IPA
DI water
| DI water
|style="background:WhiteSmoke; color:black" align="center"|
| DI water
IPA
| DI water
|style="background:WhiteSmoke; color:black" align="center"|
IPA
|style="background:WhiteSmoke; color:black" align="center"|
DI water
|style="background:WhiteSmoke; color:black" align="center"|
DI water
 
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
! scope=row style="text-align: left;" | Substrate size
|style="background:LightGrey; color:black"|Substrate size
|
|style="background:WhiteSmoke; color:black" align="center"|
* Chips
* 50 mm wafers
* 100 mm wafers
* 100 mm wafers
|style="background:WhiteSmoke; color:black" align="center"|
* 150 mm wafers
|
* Chips
* 50 mm wafers
* 100 mm wafers
* 100 mm wafers
* 150 mm wafers
* 150 mm wafers
|style="background:WhiteSmoke; color:black" align="center"|
* 200 mm wafers
* 100 mm wafers
|
|style="background:WhiteSmoke; color:black" align="center"|
* Chips (5mm to 2")
* Chips (5mm to 2")
* 50 mm wafers
* 50 mm wafers
* 100 mm wafers
* 100 mm wafers
* 150 mm wafers
* 150 mm wafers
|style="background:WhiteSmoke; color:black" align="center"|
* 200 mm wafers
|
* Chips (5mm to 2")
* Chips (5mm to 2")
* 100 mm wafers
* 100 mm wafers
* 150 mm wafers
* 150 mm wafers
|style="background:WhiteSmoke; color:black" align="center"|
|
* 100 mm wafers
* 150 mm wafers
* 200 mm wafers (may require tool change)
|
* 100 mm wafers
* 100 mm wafers
* 150 mm wafers
* 150 mm wafers
* 200 mm wafers (may require tool change)
|-
|-
|style="background:LightGrey; color:black"|Allowed materials
! scope=row style="text-align: left;" | Allowed materials
|style="background:WhiteSmoke; color:black" align="center"|
| All cleanroom approved materials
Silicon, glass, and polymer substrates
|
 
*Silicon and glass substrates
Film or pattern of all types
*Film or pattern of all but Type IV
 
| All cleanroom approved materials
|style="background:WhiteSmoke; color:black" align="center"|
|
Silicon, glass, and polymer substrates
*All cleanroom approved materials
 
*Film or pattern of all types
Film or pattern of all types
|
|style="background:WhiteSmoke; color:black" align="center"|
*Silicon and glass substrates
Silicon and glass substrates
*Films, or patterned films, of any material except type IV (Pb, Te)
 
|
Film or pattern of all but Type IV
*Silicon, III-V, and glass substrates
 
*Films, or patterned films, of any material except type IV (Pb, Te)
|style="background:WhiteSmoke; color:black" align="center"|
All cleanroom approved materials
 
|style="background:WhiteSmoke; color:black" align="center"|
All cleanroom approved materials  
 
Film or pattern of all types
|style="background:WhiteSmoke; color:black" align="center"|
Silicon and glass substrates
 
Film or pattern of all but Type IV
|-
|-
|style="background:LightGrey; color:black"|Batch
! scope=row style="text-align: left;" | Batch size
|style="background:WhiteSmoke; color:black" align="center"|
| 1 - 5
1-8
| 1 - 6
|style="background:WhiteSmoke; color:black" align="center"|
| 1
1-25
| 1
|style="background:WhiteSmoke; color:black" align="center"|
| 1 - 25
1-6
| 1 - 25
|style="background:WhiteSmoke; color:black" align="center"|
1
|style="background:WhiteSmoke; color:black" align="center"|
1
|style="background:WhiteSmoke; color:black" align="center"|
1-25  
|-  
|}
|}
<br clear="all" />
<br clear="all" />


<!-- TARAN 2020-03-05
==Developer-1 and Developer-2==
==Developer-1 and Developer-2==
[[Image:Developer1&2.jpg|300x300px|thumb|right|Developer-1 (right) and Developer-2 (left) are located in C-1]]
[[Image:Developer1&2.jpg|300x300px|thumb|right|Developer-1 (right) and Developer-2 (left) are located in C-1]]


'''Feedback to this section''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Development#Developer-1_and_Developer-2 click here]'''
'''Feedback to this section''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Development#Developer-1_and_Developer-2 click here]'''
 
===<span style="color:red">This equipment was decommissioned January 2017!</span>===


Developer-1 and Developer-2 are manual developer baths for submersion development of AZ 5214E and AZ 4562 resists in AZ 351B developer. The developer is mixed 1:5 in water by the user prior to development start, and the wafer cassette is agitated manually by the user during development. The development time is controlled manually by the user. After development, the substrates are rinsed with water in the bench.
Developer-1 and Developer-2 are manual developer baths for submersion development of AZ 5214E and AZ 4562 resists in AZ 351B developer. The developer is mixed 1:5 in water by the user prior to development start, and the wafer cassette is agitated manually by the user during development. The development time is controlled manually by the user. After development, the substrates are rinsed with water in the bench.


'''The user APV, and contact information can be found in LabManager: [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=62 Developer-1] [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=63 Developer-2]'''
'''The user APV, and contact information can be found in LabManager: [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=62 Developer-1] [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=63 Developer-2]'''


===Process information===
===Process information===
Line 309: Line 268:


<br clear="all" />
<br clear="all" />
-->


<!-- TARAN 2020-03-05
==Developer-6inch==
==Developer-6inch==


[[image:6inchDeveloper.jpg|300x300px|right|thumb|The Developer: 6inch bench is located in E-4]]
[[image:6inchDeveloper.jpg|300x300px|right|thumb|The Developer: 6inch bench is located in E-4]]


'''Feedback to this section''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Developers#Developer-6inch click here]'''
'''Feedback to this section''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Developers#Developer-6inch click here]'''
 
===<span style="color:red">This equipment will be decommissioned December 2019!</span>===


The Developer: 6inch bench is an automated developer bath for submersion development of AZ 5214E and AZ 4562 resists in AZ 351B developer. The developer is mixed 1:5 in water by the equipment prior to development start. The developer is circulated during development, and the wafer cassette may be agitated by a mechanical elevator. The development time is controlled manually by the user. After development, the substrates are rinsed with water in the bench.
The Developer: 6inch bench is an automated developer bath for submersion development of AZ 5214E and AZ 4562 resists in AZ 351B developer. The developer is mixed 1:5 in water by the equipment prior to development start. The developer is circulated during development, and the wafer cassette may be agitated by a mechanical elevator. The development time is controlled manually by the user. After development, the substrates are rinsed with water in the bench.


'''The user manual, user APV, and contact information can be found in [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=189 LabManager]'''
'''The user manual, user APV, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=189 LabManager]'''


===Process information===
===Process information===
Line 390: Line 353:


<br clear="all" />
<br clear="all" />
-->


==SU8-Developer==
==Manual beaker development in fumehood==
[[Image:SU-8developer.jpg|300x300px|right|thumb|The SU8-Developer bench is located in C-1]]
Beaker development, in fume hood 09: UV development or fume hood 10: e-beam development, is a fall-back option if you have a process, which is not compatible with the automatic, or semi-automatic, tools. We always recommend using, or at least trying, the automatic and semi-automatic tools, instead of using manual beaker development.


'''Feedback to this section''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Development#SU8-Developer click here]'''
Manual beaker development is necessary for some processes, but should be avoided if possible, due to the fact that it is notoriously difficult to get a stable repeatable process - especially when multiple users are sharing the same process; everybody simply does things a bit different from each other, which leads to changes in the process outcome. Some processes have a very narrow process window, which makes them inherently sensitive to small changes in the development. The manual development also has a much greater chance of producing particles, both from the operator and the environment.


The SU8-Developer bench is a manually operated chemical bench for submersion development of SU-8 photoresist in PGMEA (supplied in the cleanroom as mr-Dev 600). The development process is in two stages; one bath (FIRST) to dissolve the bulk of the resist, and a second, cleaner bath (FINAL) to finish the development. The development time is controlled manually by the user. After development, the substrates are rinsed with IPA and dried in the bench.
Finally the safety of the operator is at a significantly higher risk, since any manual handling of chemicals carries the risk of accidental spills with it. This is especially problematic if the developer is TMAH based, where direct skin exposure of >1% TMAH on a few percent of the body must be treated as a life-threatening event.


'''The user manual, user APV, and contact information can be found in [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=154 LabManager]'''
===Special rules for manual beaker development of TMAH===
*Automatic agitation methods are not allowed - this includes magnetic stirring or sonication
*Manual agitation methods, which create large waves or turbulence in the development solution, are not allowed
*Users must submit a risk assessment for any process requiring manual beaker development of TMAH based developers
*Users requiring manual beaker development of TMAH based developers must additionally provide valid reasons for not using the already available automatic and semi-automatic tools
 
===Standard manual beaker development procedure===
[[File:Beaker_development_v1.png|600px|thumb|Standard procedure for manual beaker development in fume hood:<br>1) Submerge exposed substrate into development solution<br>2) When timer ends, move substrate directly into Rinse 1<br>3) After a few seconds, move substrate into Rinse 2*<br>4) Remove developed substrate for drying<br>(*It is allowed to omit the Rinse 2 step)|right]]
The standard procedure for manual beaker development in a fume hood is as follows:
#Prepare development process
#Perform development
#Clean up
 
'''Prepare development process'''
*Write the chemical label, which must always be present in your chemical setup - your write your label <i>before</i> pouring the chemical
*Find the beakers required for your process
*Find the items required for holding/submerging your substrate during the process
*Find carriers or other storage units for placing your substrate after the process has finished
*Find a timer - make sure it works as you expect it to, before submerging your substrate into the development solution and discovering that the timer is in fact broken
*Get some cleanroom wipes and keep them nearby, for wiping any drops spilled during handling
*<span style="color:red">Do not cover too many of the exhaust holes in the fume hood table, as this will reduce the efficiency of the exhaust, which reduces safety</span>
*<span style="color:red">Do not place your beakers too close to the fume hood sash, as this can make it difficult to efficiently extract the fumes escaping from the beakers, which reduces safety</span>
 
'''Perform development'''
#Put on the appropriate personal protection gear
#Pour rinsing agent into Rinse 1 and Rinse 2 beakers - typically DI water or IPA
#Pour development solution into development beaker
#Place exposed substrate in the appropriate carrier
#Set timer
#Submerge substrate into development beaker
#Start timer immediately
#When timer is 5 seconds from ending, prepare to lift the substrate out of the development beaker
#Lift substrate out of development beaker - it can help to lift it at a slight angle, to allow liquids to drain more easily from large surfaces
#Submerge it immediately into Rinse 1
#Agitate up/down for at least a few seconds
#Move substrate into Rinse 2*
#Agitate slightly
#The developed substrate can now be removed and dried
 
(<nowiki>*</nowiki>It is allowed to omit the Rinse 2 step)
 
'''Clean up'''
*Pour Rinse 1 and Rinse 2 into appropriate waste: water goes into the sink, IPA goes into C-waste drain
*Rinse beakers with the DI-water gun
*Pour development solution into appropriate waste: solvent based developer goes into C-waste drain. <span style="color:red">NB! TMAH is an aqueous alkaline solution, which must never be mixed with solvents! TMAH waste goes into the dedicated TMAH waste container, stored in the chemical cabinet in E-4.</span>
*If your developer solution is not TMAH based:
**Rinse beaker 3 times, discard water into sink
*If your developer solution is TMAH based:
**Rinse beaker once with DI-water and discard this into the TMAH waste
**Rinse beaker two more times, discarding the water into the sink
*Hang all beakers to dry on the drying rack
*Erase the chemical label text
*Wipe any droplets on the fume hood surface
*Discard any napkins/other trash in the bin inside the fume hood
 
<br clear="all" />
 
==Developer: SU8 (Wet Bench)==
[[Image:SU8dev.JPG|400px|right|thumb|The Developer: SU8 (Wet Bench) is located in E-4.]]
 
The SU8-Developer bench is a manually operated wet bench for submersion development of SU-8 photoresist in PGMEA (supplied in the cleanroom as mr-Dev 600). The development process is in two stages; one bath (FIRST) to dissolve the bulk of the resist, and a second, cleaner bath (FINAL) to finish the development. The development time is controlled manually by the user. After development, the substrates are rinsed with IPA in dedicated IPA bath and put for drying in the empty bath.
 
The user manual, user APV, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=509 LabManager: Developer: SU8(Wet Bench)] - '''requires login'''


===Process information===
===Process information===
Several aspects of the outcome of SU-8 processing are affected by the development process. The lithographic resolution is affected by the time between PEB (post-exposure bake) and development, as the cross-linking process continues in the interface between exposed and unexposed regions even at room temperature. Cracks in the structures is affected by two things; the development time, and how much has previously been developed in the developer bath. Cracking is worse with longer development time, and worst in a new developer bath. The effect of the developer use quickly saturates (5-10 wafers). Finally, the stability of fine structures (high aspect ratio) is affected by the rinse after development, as the lower surface tension of IPA compared to PGMEA reduces pattern collapse during drying.
Several aspects of the outcome of SU-8 processing are affected by the development process. The lithographic resolution is affected by the time between PEB (post-exposure bake) and development, as the cross-linking process continues in the interface between exposed and unexposed regions even at room temperature. Cracks in the structures is affected by two things; the development time, and how much has previously been developed in the developer bath. Cracking is worse with longer development time, and worst in a new developer bath. The effect of the developer use quickly saturates (5-10 wafers). Finally, the stability of fine structures (high aspect ratio) is affected by the rinse after development, as the lower surface tension of IPA compared to PGMEA reduces pattern collapse during drying.


Development time is strongly dependent on the SU-8 thickness. Here are some suggestions:
 
Development time is strongly dependent on the SU-8 thickness.  
*Minimum development time: 1 min per 20 µm in FIRST
 
 
Suggestions:
*2-5µm: 2 min. in FIRST; 2 min. in FINAL
*2-5µm: 2 min. in FIRST; 2 min. in FINAL
*40µm: 5 min. in FIRST; 5 min. in FINAL (however, 3 min. in FIRST and 2 min. in FINAL is sufficient)
*40µm: 5 min. in FIRST; 5 min. in FINAL (however, 3 min. in FIRST and 2 min. in FINAL is sufficient)
Line 410: Line 441:
=== Equipment performance and process related parameters ===
=== Equipment performance and process related parameters ===


{| border="2" cellspacing="0" cellpadding="2"  
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
 


!style="background:silver; color:black;" align="center" width="60"|Purpose  
!style="background:silver; color:black;" align="center" width="60"|Purpose  
|style="background:LightGrey; color:black"|
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
Development of
Development of:
*SU-8
*SU-8
|-
|-
!style="background:silver; color:black;" align="center" width="60"|Developer  
!style="background:silver; color:black;" align="center" width="60"|Developer  
|style="background:LightGrey; color:black"|
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
mr-Dev 600
mr-Dev 600


Line 428: Line 458:
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Method
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Method
|style="background:LightGrey; color:black"|Development
|style="background:LightGrey; color:black"|Development
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
Submersion
Submersion
|-
|-
|style="background:LightGrey; color:black"|Handling
|style="background:LightGrey; color:black"|Handling
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
Single wafer holder
Single wafer holder
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Process parameters
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Process parameters
|style="background:LightGrey; color:black"|Temperature
|style="background:LightGrey; color:black"|Temperature
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
Room temperature
Room temperature
|-
|-
|style="background:LightGrey; color:black"|Agitation
|style="background:LightGrey; color:black"|Agitation
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
Magnetic stirrer
Magnetic stirrer
|-
|-
|style="background:LightGrey; color:black"|Rinse
|style="background:LightGrey; color:black"|Rinse
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
IPA
IPA
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
|style="background:LightGrey; color:black"|Substrate size
|style="background:LightGrey; color:black"|Substrate size
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
* 100 mm wafers
*100 mm wafers
150 mm wafer is possible if the level is high enough
*150 mm wafers, check the liquid level in the baths
*200 mm wafer, check the liquid level in the baths
|-
|-
| style="background:LightGrey; color:black"|Allowed materials
| style="background:LightGrey; color:black"|Allowed materials
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
Silicon and glass substrates
*Silicon and glass substrates
 
*Film, or pattern, of all materials except Type IV
Film or pattern of all but Type IV
|-
|-
|style="background:LightGrey; color:black"|Batch
|style="background:LightGrey; color:black"|Batch
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
1-6  
1-6  
|-  
|-  
Line 468: Line 498:
<br clear="all" />
<br clear="all" />


==Developer: E-beam Manual==
==Developer: E-beam 02==
[[Image:IMG 2464.JPG|300×300px|right|thumb|Developer: E-beam Manual is located in E-4]]
[[Image:IMG 2464.JPG|400px|right|thumb|Developer: E-beam 02 is located in E-4.]]
 
'''Feedback to this section''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Development#Developer:_TMAH_Manual click here]'''
 
Developer: E-beam Manual is a manually operated, single substrate or chip spray-puddle developer. It uses the N50 or AR 600-546 developers and IPA for rinsing. The substrates or chips are loaded manually one by one into the developer. Developer dispense, puddle time, water rinse, and drying is performed automatically by the equipment.


The machine is setup to agitate and be stationary to enhance the development uniformity - this is a ongoing process.
Developer: E-beam 02 is a manually operated, single substrate puddle developer. It uses the ZED-N50 or AR 600-50 developers and IPA for rinsing. The substrates are loaded manually one by one into the developer. Developer dispense, puddle time, IPA rinse, and drying is then performed automatically by the equipment.


'''[http://podcast.llab.dtu.dk/fileadmin/podcasts/2016/DTUDanchip/1.049_Developer_Manual-720p.mp4 Training video]'''
'''[https://www.youtube.com/watch?v=btinNzYnLnY Training video]''' (for Developer: TMAH Manual, but it is the same model)


'''The user manual, user APV, and contact information can be found in [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=324 LabManager]'''
The user manual, user APV, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=324 LabManager] - '''requires login'''


===Process information===
===Process information===
All recipes use the following structure:
#Pressurize the developer canister
#Dispense puddle while rotating substrate slowly
#Puddle development while not rotating
#Agitate substrate once per 15 seconds by rotating slowly for 1 second
#Spin off developer
#Clean substrate with IPA
#Dry substrate and chamber with nitrogen


All recipes are single puddle.
Multi-puddle recipes repeat steps 2-5 for the given number of puddles.
N50 and 546 denotes the developer used (546 is short for AR 600- 546).
The first step is pressurizing the canister so nothing will happen visually.
Please watch if the developer and rinsing starts. If not try to restart the machine by pressing the EMO and turning it on again.
The spray is 8-10 s and will start the development process hence the short recipes (10s and 30s.) have been adjusted according to this.
6" have some uniformity issues but the recipes are being modified to compensate for this.


'''Process recipes'''
*546 10s: 10s. Development Rinse and dry.
*546 30s: 60s. Development Rinse and dry.
*546 60s: 120s. Development Rinse and dry.
*N50 10s: 10s. Development Rinse and dry.
*N50 30s: 30s. Development Rinse and dry.
*N50 60s: 60s. Development Rinse and dry.
*N50 90s: 90s. Development Rinse and dry.
*N50 120s: 120s. Development Rinse and dry.
*N50 180s: 180s. Development Rinse and dry.
*N50 180s6": Test for changing the agitation for 6" uniformity 180s. Development Rinse and dry.
*Testdev: The time can be modified 60s. Development Rinse and dry on AR 600-546.
*Rinse: Rinse and dry.


'''Utility recipes'''
'''Process recipes'''<br>
*UTIL-DR: Dome rinse.
N50 recipes have the letter "N" in them. AR-600-50 recipes have the letter "A"  in them. The number is the development time in seconds:
*UTIL-BE: Bottle empty. Danchip use only.
*01 Rinse
*02 N 15
*03 N 30
*04 N 60
*05 N 90
*06 N 120
*07 N 180
*08 N 300
*09 N 600
*10 N 2x60
*11 N 5x60
*12 A 15
*13 A 30
*14 A 60
*15 A 90
*16 A 120
*17 A 180
*18 A 300
*19 A 600
*20 A 2x60
*21 A 5x60


=== Equipment performance and process related parameters ===
=== Equipment performance and process related parameters ===


{| border="2" cellspacing="0" cellpadding="2"  
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  


|-
|-
!style="background:silver; color:black;" align="center" width="60"|Purpose  
!style="background:silver; color:black;" align="center" width="60"|Purpose  
|style="background:LightGrey; color:black"|
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
Development of
Development of:
*CSAR
*CSAR
*ZEP520A
*ZEP520A


|-
|-
!style="background:silver; color:black;" align="center" width="60"|Developer  
!style="background:silver; color:black;" width="60"|Developer  
|style="background:LightGrey; color:black"|
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
*AR 600-546 (546)
*AR 600-50
*N-50
*ZED N-50
 
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Method
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Method
|style="background:LightGrey; color:black"|Development
|style="background:LightGrey; color:black"|Development
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
Spray/Puddle
Puddle
|-
|-
|style="background:LightGrey; color:black"|Handling
|style="background:LightGrey; color:black"|Handling
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
Vacuum chuck for 2",4" or 6" wafers and chip "basket"
*Chip chuck for chips
*Non-vacuum chuck for 2" wafers
*Non-vacuum chuck for 100 mm and 150 mm wafers
*Non-vacuum chuck for 200 mm wafers
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Process parameters
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Process parameters
|style="background:LightGrey; color:black"|Temperature
|style="background:LightGrey; color:black"|Temperature
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
Room temperature
Room temperature
|-
|-
|style="background:LightGrey; color:black"|Agitation
|style="background:LightGrey; color:black"|Agitation
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
Yes 15rpm back and forth
1 second rotational agitation at 30 rpm every 15 seconds
|-
|-
|style="background:LightGrey; color:black"|Rinse
|style="background:LightGrey; color:black"|Rinse
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
IPA - Isopropanol
IPA
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
|style="background:LightGrey; color:black"|Substrate size
|style="background:LightGrey; color:black"|Substrate size
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
* Chips (6-60 mm)
*Chips
* 50 mm wafers
*2" wafers
* 100 mm wafers
*100 mm wafers
* 150 mm wafers
*150 mm wafers
*200 mm wafers
|-
|-
| style="background:LightGrey; color:black"|Allowed materials
| style="background:LightGrey; color:black"|Allowed materials
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
All cleanroom approved materials  
*All cleanroom approved materials  
 
*Film, or pattern, of all materials except Type IV
Film or pattern of all types
|-
|-
|style="background:LightGrey; color:black"|Batch
|style="background:LightGrey; color:black"|Batch size
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
1  
1  
|-  
|-  
Line 572: Line 610:
<br clear="all" />
<br clear="all" />


==Developer: TMAH Manual==
==Developer: TMAH Manual 02==
[[Image:IMG 2464.JPG|300×300px|right|thumb|Developer: TMAH Manual is located in E-4]]
[[Image:IMG 2464.JPG|400px|right|thumb|Developer: TMAH Manual 02 is located in E-4.]]


'''Feedback to this section''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Development#Developer:_TMAH_Manual click here]'''
Developer: TMAH Manual 02 is a manually operated, single substrate or chip puddle developer. It uses the TMAH based AZ 726 MIF developer (2.38 % TMAH in  water with a small amount of wetting agent). The substrates or chips are loaded manually one by one into the developer. Developer dispense, puddle time, water rinse, and drying is performed automatically by the equipment.


Developer: TMAH Manual is a manually operated, single substrate or chip spray-puddle developer. It uses the TMAH based AZ 726 MIF developer (2.38 % TMAH in  water with a small amount of wetting agent). The substrates or chips are loaded manually one by one into the developer. Developer dispense, puddle time, water rinse, and drying is performed automatically by the equipment.


The spray nozzle makes it difficult to build up a perfect puddle on 4" or 6" substrates which affects the effectiveness and uniformity of the development. Pre-wetting during dispense or agitation during development may give better results.
'''[https://www.youtube.com/watch?v=btinNzYnLnY Training video]'''


'''[http://podcast.llab.dtu.dk/fileadmin/podcasts/2016/DTUDanchip/1.049_Developer_Manual-720p.mp4 Training video]'''


'''The user manual, user APV, and contact information can be found in [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=324 LabManager]'''
The user manual, user APV, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=324 LabManager] - '''requires login'''


===Process information===
===Process information===
All recipes use the following structure:
#Pressurize the TMAH canister
#Dispense puddle while rotating substrate slowly
#Puddle development while not rotating
#Agitate substrate once per 15 seconds by rotating slowly for 1 second
#Spin off developer
#Clean substrate and chamber with DI water
#Dry substrate and chamber with nitrogen
Multi-puddle recipes repeat steps 2-5 for the given number of puddles.


'''Process recipes'''
'''Process recipes'''<br>
*DP 2x60s: Double puddle, 2 times 60s. Rinse and dry.
SP: Single-puddle<br>
*MP 4x60s: Multiple puddle, 4 times 60s. Rinse and dry.
MP: Multi-puddle
*SP 120s: Single puddle, 120s. Rinse and dry.
*SP 15s: Single puddle, 15s. Rinse and dry.
*SP 30s: Single puddle, 30s. Rinse and dry.
*SP 60s: Single puddle, 60s. Rinse and dry.


'''Utility recipes'''
*01 Rinse
*UTIL-DR: Dome rinse.
*02 SP 15
*UTIL-BE: Bottle empty. Danchip use only.
*03 SP 30
*04 SP 60
*05 SP 90
*06 SP 120
*07 SP 300
*08 MP 2x60
*09 MP 5x60
*91 SP test
*92 MP test


=== Equipment performance and process related parameters ===
=== Equipment performance and process related parameters ===


{| border="2" cellspacing="0" cellpadding="2"  
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  




!style="background:silver; color:black;" align="center" width="60"|Purpose  
!style="background:silver; color:black;" align="center" width="60"|Purpose  
|style="background:LightGrey; color:black"|
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
Development of
Development of UV resists:
*AZ nLOF
*AZ nLOF
*AZ MiR 701
*AZ MiR 701
*AZ 5214E
*AZ 5214E
*AZ 4562
*AZ 4562
*DUV resists
Development of DUV resists:
*KRF M230Y
*KRF M35G
|-
|-
!style="background:silver; color:black;" align="center" width="60"|Developer  
!style="background:silver; color:black;" align="center" width="60"|Developer  
|style="background:LightGrey; color:black"|
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
AZ 726 MIF
AZ 726 MIF<br>
 
(2.38% TMAH in water)
(2.38% TMAH in water)
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Method
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Method
|style="background:LightGrey; color:black"|Development
|style="background:LightGrey; color:black"|Development
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
Spray/Puddle
Puddle
|-
|-
|style="background:LightGrey; color:black"|Handling
|style="background:LightGrey; color:black"|Handling
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
Edge handling chuck or chip "basket"
*Chip chuck for chips and 2" wafers
*Non-vacuum chuck for 100 mm and 150 mm wafers
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Process parameters
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Process parameters
|style="background:LightGrey; color:black"|Temperature
|style="background:LightGrey; color:black"|Temperature
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
Room temperature
Room temperature
|-
|-
|style="background:LightGrey; color:black"|Agitation
|style="background:LightGrey; color:black"|Agitation
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
none
1 second rotational agitation at 30 rpm every 15 seconds
|-
|-
|style="background:LightGrey; color:black"|Rinse
|style="background:LightGrey; color:black"|Rinse
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
DI water
DI water
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
|style="background:LightGrey; color:black"|Substrate size
|style="background:LightGrey; color:black"|Substrate size
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
* Chips (6-60 mm)
*Chips (6-60 mm)
* 100 mm wafers
*100 mm wafers
* 150 mm wafers
*150 mm wafers
|-
|-
| style="background:LightGrey; color:black"|Allowed materials
| style="background:LightGrey; color:black"|Allowed materials
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
All cleanroom approved materials  
*All cleanroom approved materials  
 
*Film, or pattern, of all materials except Type IV
Film or pattern of all types
|-
|-
|style="background:LightGrey; color:black"|Batch
|style="background:LightGrey; color:black"|Batch size
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
1  
1
|-  
|-  
|}
|}
<br clear="all" />
<br clear="all" />


==Developer TMAH UV-lithography==
==Developer TMAH UV-lithography==


[[Image:SUSS DEV.JPG|300x300px|right|thumb|Developer: TMAH UV-lithography is located in E-4]]
[[Image:SUSS DEV.JPG|400px|right|thumb|Developer: TMAH UV-lithography is located in E-4.]]
 
Developer TMAH UV-lithography was released Q4 2014.


'''Feedback to this section''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Development#Developer_TMAH_UV-lithography click here]'''
Link to information about [[Specific_Process_Knowledge/Pattern_Design#Helpful_information_for_chip_layout|developer chuck size and hotplate pin positions]].


Developer TMAH UV-lithography was released Q4 2014.
'''[https://www.youtube.com/watch?v=fs9DRH0Eo3k Training video]'''


'''[http://podcast.llab.dtu.dk/fileadmin/podcasts/2016/DTUDanchip/1.050_Developer_TMAH_UV-Lithography-720p.mp4 Training video]'''


'''The user manual, user APV, and contact information can be found in [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=329 LabManager]'''
The user manual, user APV, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=329 LabManager] - '''requires login'''


===Process information===
===[[Specific Process Knowledge/Lithography/Development/Developer TMAH UV-lithography processing|Process Information]]===
*[[Specific Process Knowledge/Lithography/Development/Developer TMAH UV-lithography processing|General process information]]
*[[Specific Process Knowledge/Lithography/Development/Developer_TMAH_UV-lithography_processing#General_Process_Information|General process information]]
*[[Specific Process Knowledge/Lithography/Development/Developer TMAH UV-lithography_processing#Process recommendations|Process recommendations]]
*[[Specific Process Knowledge/Lithography/Development/Developer TMAH UV-lithography_processing#Process recommendations|Process recommendations]]
*[[Specific Process Knowledge/Lithography/Development/Developer TMAH UV-lithography processing#Standard Processes|Standard processes]]
*[[Specific Process Knowledge/Lithography/Development/Developer TMAH UV-lithography processing#Standard Processes|Standard processes]]
Line 683: Line 735:
=== Equipment performance and process related parameters ===
=== Equipment performance and process related parameters ===


{| border="2" cellspacing="0" cellpadding="2"  
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  


!style="background:silver; color:black;" align="center" width="60"|Purpose  
!style="background:silver; color:black;" width="60"|Purpose  
|style="background:LightGrey; color:black"|
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
Development of
Development of
*AZ nLOF
*AZ nLOF
Line 695: Line 747:
*DUV resists
*DUV resists
|-
|-
!style="background:silver; color:black;" align="center" width="60"|Developer  
!style="background:silver; color:black;" width="60"|Developer  
|style="background:LightGrey; color:black"|
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black" |
AZ 726 MIF
AZ 726 MIF


Line 704: Line 756:
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Method
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Method
|style="background:LightGrey; color:black"|Development
|style="background:LightGrey; color:black"|Development
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
Puddle
Puddle
|-
|-
|style="background:LightGrey; color:black"|Handling
|style="background:LightGrey; color:black"|Handling
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
Vacuum chuck
Vacuum chuck
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Process parameters
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Process parameters
|style="background:LightGrey; color:black"|Temperature
|style="background:LightGrey; color:black"|Temperature
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
Room temperature
Room temperature
|-
|-
|style="background:LightGrey; color:black"|Agitation
|style="background:LightGrey; color:black"|Agitation
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
Rotation
Rotation
|-
|-
|style="background:LightGrey; color:black"|Rinse
|style="background:LightGrey; color:black"|Rinse
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
DI water
DI water
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
|style="background:LightGrey; color:black"|Substrate size
|style="background:LightGrey; color:black"|Substrate size
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
* 100 mm wafers
* 100 mm wafers
* 150 mm wafers
* 150 mm wafers
|-
|-
| style="background:LightGrey; color:black"|Allowed materials
| style="background:LightGrey; color:black"|Allowed materials
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
Silicon and glass substrates
Silicon and glass substrates


Line 737: Line 789:
|-
|-
|style="background:LightGrey; color:black"|Batch
|style="background:LightGrey; color:black"|Batch
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
1-25  
1-25  
|-  
|-  
|}
|}
<br clear="all" />


<br clear="all" />
{{:Specific Process Knowledge/Lithography/Development/DUV_developer}}

Latest revision as of 15:52, 2 April 2025

The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.

Feedback to this page: click here

Development Comparison Table

Manual beaker development Developer: SU8 (Wet bench) Developer: E-beam 02 Developer: TMAH Manual 02 Developer: TMAH UV-lithography Developer: TMAH Stepper
Purpose

Fall-back option if you have a process, which is not compatible with the automatic, or semi-automatic, tools

Requires individual risk assessment for TMAH development!

Development of:

  • SU-8

Development of:

  • ZEP 520A
  • AR-P 6200.xx (CSAR)

Development of:

  • AZ nLOF
  • AZ MiR 701
  • AZ 5214E
  • AZ 4562
  • DUV resists

Development of:

  • AZ nLOF
  • AZ MiR 701
  • AZ 5214E
  • AZ 4562
  • DUV resists

Post-exposure baking

Development of:

  • DUV resists

Post-exposure baking

Developer Process dependent mr-Dev 600 (PGMEA)
  • ZED N-50
  • AR 600-50
AZ 726 MIF (2.38% TMAH in water) AZ 726 MIF (2.38% TMAH in water) AZ 726 MIF (2.38% TMAH in water)
Method Submersion Submersion Puddle Puddle Puddle Puddle
Handling

Manual handling in beakers

  • Chip bucket
  • Single wafer carrier
  • Carrier for up to 5 wafers
  • Chip bucket
  • Single wafer carrier
  • Carrier for up to 6 wafers
  • Vacuum-free edge-grip chucks for 50 mm, 100 mm & 150 mm, and 200 mm substrates
  • Chip chuck for chips & 2" substrates
  • Vacuum-free edge-grip chucks for 50 mm, 100 mm & 150 mm, and 200 mm substrates
  • Chip chuck for chips & 2" substrates
Vacuum chuck Vacuum chuck
Process temperature Room temperature Room temperature Room temperature Room temperature Room temperature Room temperature
Process agitation No agitation allowed Magnetic stirrer Rotation Rotation Rotation Rotation
Process rinse Process dependent IPA IPA DI water DI water DI water
Substrate size
  • Chips
  • 50 mm wafers
  • 100 mm wafers
  • 150 mm wafers
  • Chips
  • 50 mm wafers
  • 100 mm wafers
  • 150 mm wafers
  • 200 mm wafers
  • Chips (5mm to 2")
  • 50 mm wafers
  • 100 mm wafers
  • 150 mm wafers
  • 200 mm wafers
  • Chips (5mm to 2")
  • 100 mm wafers
  • 150 mm wafers
  • 100 mm wafers
  • 150 mm wafers
  • 200 mm wafers (may require tool change)
  • 100 mm wafers
  • 150 mm wafers
  • 200 mm wafers (may require tool change)
Allowed materials All cleanroom approved materials
  • Silicon and glass substrates
  • Film or pattern of all but Type IV
All cleanroom approved materials
  • All cleanroom approved materials
  • Film or pattern of all types
  • Silicon and glass substrates
  • Films, or patterned films, of any material except type IV (Pb, Te)
  • Silicon, III-V, and glass substrates
  • Films, or patterned films, of any material except type IV (Pb, Te)
Batch size 1 - 5 1 - 6 1 1 1 - 25 1 - 25



Manual beaker development in fumehood

Beaker development, in fume hood 09: UV development or fume hood 10: e-beam development, is a fall-back option if you have a process, which is not compatible with the automatic, or semi-automatic, tools. We always recommend using, or at least trying, the automatic and semi-automatic tools, instead of using manual beaker development.

Manual beaker development is necessary for some processes, but should be avoided if possible, due to the fact that it is notoriously difficult to get a stable repeatable process - especially when multiple users are sharing the same process; everybody simply does things a bit different from each other, which leads to changes in the process outcome. Some processes have a very narrow process window, which makes them inherently sensitive to small changes in the development. The manual development also has a much greater chance of producing particles, both from the operator and the environment.

Finally the safety of the operator is at a significantly higher risk, since any manual handling of chemicals carries the risk of accidental spills with it. This is especially problematic if the developer is TMAH based, where direct skin exposure of >1% TMAH on a few percent of the body must be treated as a life-threatening event.

Special rules for manual beaker development of TMAH

  • Automatic agitation methods are not allowed - this includes magnetic stirring or sonication
  • Manual agitation methods, which create large waves or turbulence in the development solution, are not allowed
  • Users must submit a risk assessment for any process requiring manual beaker development of TMAH based developers
  • Users requiring manual beaker development of TMAH based developers must additionally provide valid reasons for not using the already available automatic and semi-automatic tools

Standard manual beaker development procedure

Standard procedure for manual beaker development in fume hood:
1) Submerge exposed substrate into development solution
2) When timer ends, move substrate directly into Rinse 1
3) After a few seconds, move substrate into Rinse 2*
4) Remove developed substrate for drying
(*It is allowed to omit the Rinse 2 step)

The standard procedure for manual beaker development in a fume hood is as follows:

  1. Prepare development process
  2. Perform development
  3. Clean up

Prepare development process

  • Write the chemical label, which must always be present in your chemical setup - your write your label before pouring the chemical
  • Find the beakers required for your process
  • Find the items required for holding/submerging your substrate during the process
  • Find carriers or other storage units for placing your substrate after the process has finished
  • Find a timer - make sure it works as you expect it to, before submerging your substrate into the development solution and discovering that the timer is in fact broken
  • Get some cleanroom wipes and keep them nearby, for wiping any drops spilled during handling
  • Do not cover too many of the exhaust holes in the fume hood table, as this will reduce the efficiency of the exhaust, which reduces safety
  • Do not place your beakers too close to the fume hood sash, as this can make it difficult to efficiently extract the fumes escaping from the beakers, which reduces safety

Perform development

  1. Put on the appropriate personal protection gear
  2. Pour rinsing agent into Rinse 1 and Rinse 2 beakers - typically DI water or IPA
  3. Pour development solution into development beaker
  4. Place exposed substrate in the appropriate carrier
  5. Set timer
  6. Submerge substrate into development beaker
  7. Start timer immediately
  8. When timer is 5 seconds from ending, prepare to lift the substrate out of the development beaker
  9. Lift substrate out of development beaker - it can help to lift it at a slight angle, to allow liquids to drain more easily from large surfaces
  10. Submerge it immediately into Rinse 1
  11. Agitate up/down for at least a few seconds
  12. Move substrate into Rinse 2*
  13. Agitate slightly
  14. The developed substrate can now be removed and dried

(*It is allowed to omit the Rinse 2 step)

Clean up

  • Pour Rinse 1 and Rinse 2 into appropriate waste: water goes into the sink, IPA goes into C-waste drain
  • Rinse beakers with the DI-water gun
  • Pour development solution into appropriate waste: solvent based developer goes into C-waste drain. NB! TMAH is an aqueous alkaline solution, which must never be mixed with solvents! TMAH waste goes into the dedicated TMAH waste container, stored in the chemical cabinet in E-4.
  • If your developer solution is not TMAH based:
    • Rinse beaker 3 times, discard water into sink
  • If your developer solution is TMAH based:
    • Rinse beaker once with DI-water and discard this into the TMAH waste
    • Rinse beaker two more times, discarding the water into the sink
  • Hang all beakers to dry on the drying rack
  • Erase the chemical label text
  • Wipe any droplets on the fume hood surface
  • Discard any napkins/other trash in the bin inside the fume hood


Developer: SU8 (Wet Bench)

The Developer: SU8 (Wet Bench) is located in E-4.

The SU8-Developer bench is a manually operated wet bench for submersion development of SU-8 photoresist in PGMEA (supplied in the cleanroom as mr-Dev 600). The development process is in two stages; one bath (FIRST) to dissolve the bulk of the resist, and a second, cleaner bath (FINAL) to finish the development. The development time is controlled manually by the user. After development, the substrates are rinsed with IPA in dedicated IPA bath and put for drying in the empty bath.

The user manual, user APV, and contact information can be found in LabManager: Developer: SU8(Wet Bench) - requires login

Process information

Several aspects of the outcome of SU-8 processing are affected by the development process. The lithographic resolution is affected by the time between PEB (post-exposure bake) and development, as the cross-linking process continues in the interface between exposed and unexposed regions even at room temperature. Cracks in the structures is affected by two things; the development time, and how much has previously been developed in the developer bath. Cracking is worse with longer development time, and worst in a new developer bath. The effect of the developer use quickly saturates (5-10 wafers). Finally, the stability of fine structures (high aspect ratio) is affected by the rinse after development, as the lower surface tension of IPA compared to PGMEA reduces pattern collapse during drying.


Development time is strongly dependent on the SU-8 thickness.

  • Minimum development time: 1 min per 20 µm in FIRST


Suggestions:

  • 2-5µm: 2 min. in FIRST; 2 min. in FINAL
  • 40µm: 5 min. in FIRST; 5 min. in FINAL (however, 3 min. in FIRST and 2 min. in FINAL is sufficient)
  • 180-250µm: 15 min. in FIRST; 15 min. in FINAL

Equipment performance and process related parameters

Purpose

Development of:

  • SU-8
Developer

mr-Dev 600

(PGMEA)

Method Development

Submersion

Handling

Single wafer holder

Process parameters Temperature

Room temperature

Agitation

Magnetic stirrer

Rinse

IPA

Substrates Substrate size
  • 100 mm wafers
  • 150 mm wafers, check the liquid level in the baths
  • 200 mm wafer, check the liquid level in the baths
Allowed materials
  • Silicon and glass substrates
  • Film, or pattern, of all materials except Type IV
Batch

1-6


Developer: E-beam 02

Developer: E-beam 02 is located in E-4.

Developer: E-beam 02 is a manually operated, single substrate puddle developer. It uses the ZED-N50 or AR 600-50 developers and IPA for rinsing. The substrates are loaded manually one by one into the developer. Developer dispense, puddle time, IPA rinse, and drying is then performed automatically by the equipment.

Training video (for Developer: TMAH Manual, but it is the same model)

The user manual, user APV, and contact information can be found in LabManager - requires login

Process information

All recipes use the following structure:

  1. Pressurize the developer canister
  2. Dispense puddle while rotating substrate slowly
  3. Puddle development while not rotating
  4. Agitate substrate once per 15 seconds by rotating slowly for 1 second
  5. Spin off developer
  6. Clean substrate with IPA
  7. Dry substrate and chamber with nitrogen

Multi-puddle recipes repeat steps 2-5 for the given number of puddles.


Process recipes
N50 recipes have the letter "N" in them. AR-600-50 recipes have the letter "A" in them. The number is the development time in seconds:

  • 01 Rinse
  • 02 N 15
  • 03 N 30
  • 04 N 60
  • 05 N 90
  • 06 N 120
  • 07 N 180
  • 08 N 300
  • 09 N 600
  • 10 N 2x60
  • 11 N 5x60
  • 12 A 15
  • 13 A 30
  • 14 A 60
  • 15 A 90
  • 16 A 120
  • 17 A 180
  • 18 A 300
  • 19 A 600
  • 20 A 2x60
  • 21 A 5x60

Equipment performance and process related parameters

Purpose

Development of:

  • CSAR
  • ZEP520A
Developer
  • AR 600-50
  • ZED N-50
Method Development

Puddle

Handling
  • Chip chuck for chips
  • Non-vacuum chuck for 2" wafers
  • Non-vacuum chuck for 100 mm and 150 mm wafers
  • Non-vacuum chuck for 200 mm wafers
Process parameters Temperature

Room temperature

Agitation

1 second rotational agitation at 30 rpm every 15 seconds

Rinse

IPA

Substrates Substrate size
  • Chips
  • 2" wafers
  • 100 mm wafers
  • 150 mm wafers
  • 200 mm wafers
Allowed materials
  • All cleanroom approved materials
  • Film, or pattern, of all materials except Type IV
Batch size

1


Developer: TMAH Manual 02

Developer: TMAH Manual 02 is located in E-4.

Developer: TMAH Manual 02 is a manually operated, single substrate or chip puddle developer. It uses the TMAH based AZ 726 MIF developer (2.38 % TMAH in water with a small amount of wetting agent). The substrates or chips are loaded manually one by one into the developer. Developer dispense, puddle time, water rinse, and drying is performed automatically by the equipment.


Training video


The user manual, user APV, and contact information can be found in LabManager - requires login

Process information

All recipes use the following structure:

  1. Pressurize the TMAH canister
  2. Dispense puddle while rotating substrate slowly
  3. Puddle development while not rotating
  4. Agitate substrate once per 15 seconds by rotating slowly for 1 second
  5. Spin off developer
  6. Clean substrate and chamber with DI water
  7. Dry substrate and chamber with nitrogen

Multi-puddle recipes repeat steps 2-5 for the given number of puddles.


Process recipes
SP: Single-puddle
MP: Multi-puddle

  • 01 Rinse
  • 02 SP 15
  • 03 SP 30
  • 04 SP 60
  • 05 SP 90
  • 06 SP 120
  • 07 SP 300
  • 08 MP 2x60
  • 09 MP 5x60
  • 91 SP test
  • 92 MP test

Equipment performance and process related parameters

Purpose

Development of UV resists:

  • AZ nLOF
  • AZ MiR 701
  • AZ 5214E
  • AZ 4562

Development of DUV resists:

  • KRF M230Y
  • KRF M35G
Developer

AZ 726 MIF
(2.38% TMAH in water)

Method Development

Puddle

Handling
  • Chip chuck for chips and 2" wafers
  • Non-vacuum chuck for 100 mm and 150 mm wafers
Process parameters Temperature

Room temperature

Agitation

1 second rotational agitation at 30 rpm every 15 seconds

Rinse

DI water

Substrates Substrate size
  • Chips (6-60 mm)
  • 100 mm wafers
  • 150 mm wafers
Allowed materials
  • All cleanroom approved materials
  • Film, or pattern, of all materials except Type IV
Batch size

1


Developer TMAH UV-lithography

Developer: TMAH UV-lithography is located in E-4.

Developer TMAH UV-lithography was released Q4 2014.

Link to information about developer chuck size and hotplate pin positions.

Training video


The user manual, user APV, and contact information can be found in LabManager - requires login

Process Information

Equipment performance and process related parameters

Purpose

Development of

  • AZ nLOF
  • AZ MiR 701
  • AZ 5214E
  • AZ 4562
  • DUV resists
Developer

AZ 726 MIF

(2.38% TMAH in water)

Method Development

Puddle

Handling

Vacuum chuck

Process parameters Temperature

Room temperature

Agitation

Rotation

Rinse

DI water

Substrates Substrate size
  • 100 mm wafers
  • 150 mm wafers
Allowed materials

Silicon and glass substrates

Film or pattern of all except Type IV

Batch

1-25


Developer: TMAH Stepper

The Developer-TMAH-Stepper is placed in F-3.

This developer is dedicated for development of DUV resists. The developer is fully automatic and can run up to 25 substrates in a batch 4", 6", and 8" size (8" requires tool change). The machine is equipped with 1 developer line, in our case 2,38% TMAH in water (AZ 726 MIF), 1 topside rinse line with water, 1 backside rinse line with water and 1 N2 line for drying.


The user manual and contact information can be found in LabManager - requires login


Process information

The SEM picture of 250 nm pillars and lines. Exposure dose is 140 J/m2.

The development process will be performed by the customer together with the Photolith group of DTU Nanolab. In case you would like to do DUV lithography please contact Lithography team, who will consult you and run your wafers together with you.

Here you can find a chart‎ demonstrating a dependence between 250 nm line width/pillars diameter and exposure dose.

Standard processes

Post-exposure bake sequences:

  • (1000) DCH PEB 130C 60s 60s baking at 130°C; 20s cooling
  • (1001) DCH PEB 130C 90s 90s baking at 130°C; 20s cooling

Development sequences:

  • (1004) DCH DEV 60s 60s single puddle development

Combined PEB and development sequences:

  • (1002) DCH PEB_60s and DEV_60s 60s baking at 130°C followed by 60s single puddle development
  • (1003) DCH PEB_90s and DEV_60s 90s baking at 130°C followed by 60s single puddle development

The standard developer process consists of:

  • pre-wetting with water (2.5s @ 1000rpm)
  • developer dispense (2.5s @ 40rpm, corresponding to ~9ml)
  • development (60s @ 0rpm)
  • water rinse with BSR (5s @ 3000rpm)
  • nitrogen drying (7s @ 4000rpm)

and has a cycle time of ~2 minutes


Equipment performance and process related parameters

Purpose

Development of DUV resist: KRF M230Y and KRF M35G

Developer

2,38% water based TMAH

Process parameters Spin speed

10 - 5000 rpm

Spin acceleration

100 - 10000 rpm/s

Hotplate temperature

130°C for post exposure baking

Substrates Substrate size
  • 100 mm wafers
  • 150 mm wafers
  • 200 mm wafers (requires tool change)
Allowed materials
  • Any standard cleanroom material
Batch

1 - 25