Jump to content

Specific Process Knowledge/Lithography/Coaters/Spin Coater: RCD8 processing: Difference between revisions

From LabAdviser
Taran (talk | contribs)
Created page with "=Spin coating= The process of spin coating on Spin Track 1 + 2 consists of a selection of the following steps: *Acceleration to a low spin speed if dynamic dispense is used *R..."
 
Taran (talk | contribs)
(108 intermediate revisions by 3 users not shown)
Line 1: Line 1:
{{:Specific Process Knowledge/Lithography/authors_generic}}
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Lithography/Coaters/Spin_Coater:_RCD8_processing click here]'''
[[Category: Equipment|Lithography]]
[[Category: Lithography]]
__TOC__
=Spin coating=
=Spin coating=
The process of spin coating on Spin Track 1 + 2 consists of a selection of the following steps:
Spin coating on Spin Coater: RCD8 consists of a selection of the following steps:
*Acceleration to a low spin speed if dynamic dispense is used
#Optional: Acceleration to a low spin speed if dynamic dispense is used
*Resist dispense
#Resist dispense
*Resist spreading at low spin speed
#Optional: Closing the Gyrset (if used)
*Spin-off
#Optional: Resist spreading at low spin speed
*Deceleration before stop or further process steps
#Spin-off
*Edge-bead removal using PGMEA
#Deceleration
*Backside rinse using PGMEA
#Opening Gyrset
 
 
The wafer is first centered on the chuck and held in place by vacuum (or pins in the case of the non-vacuum chuck). If static dispense is used, the spindle remains static during the ensuing resist dispense. In the case of dynamic dispense, the spindle is accelerated to a low spin speed before the resist is dispensed. Using too high spin speed during dispense can cause surface wetting issues, while a too low spin speed causes the resist to flow onto the backside of the wafer. The resist may be dispensed manually, or automatically using the syringe dispense system on the media arm. After dispense, a short spin at low spin speed may be used in order to spread the resist over the wafer surface before spin-off.
 
The spin-off cycle determines the thickness of the resist coating. The thickness is primarily a function of the spin-off speed and the spin-off time, both following an inverse power-law.
The acceleration to the spin-off speed also influences the thickness, but the effect is dependent on previous steps. The spin-off is usually a simple spin at one speed, but it may be comprised of several steps at different spin speeds. After spin-off, the wafer is decelerated.
 
=Automatic dispense=
 
Automatic dispense on the Spin Coater: RCD8 is done using a Nordson EFD Performus VII pressurised cartridge dispense system. The syringe containing the resist is mounted on the media arm, and the resist is dispensed using a nitrogen pressure supplied by the control box. The dispense rate is controlled by the nitrogen pressure, while the dispense time, and thus the volume, is set in the recipe. The dispensed volume may be estimated by measuring the distance the resist level is displaced during a dispense, and calculating the corresponding volume using the diameter of the syringe (23 mm). A displacement of 10 mm corresponds to a dispensed volume of 4 mL.
 
Observed dispense rates (uncertainty from measurements ~0.1 ml/s):
*'''SU-8 2075:'''
**0.2 ml/s @ 1.0 bar
**0.5 ml/s @ 2.0 bar
**0.7 ml/s @ 3.0 bar
*'''SU-8 2035:'''
**0.5 ml/s @ 1.0 bar
*'''SU-8 2010:'''
**1.1 ml/s @ 0.1 bar
*'''KMPR 1025:'''
**0.4 ml/s @ 0.5 bar
**0.7 ml/s @ 1.0 bar
*'''AZ 5214E:'''
**1.2 ml/s @ 0.1 bar
**2.4 ml/s @ 0.18 bar
 
==Edge bead removal==
The automatic dispense system may also be used to administer solvent at the edge of the wafer after spin coating in order to remove the edge bead. Edge bead removal, or EBR, is usually done using PGMEA. Due to the low viscosity of the solvent, and the relatively high pressure of the EFD control box, it is necessary to use at tip at the end of the syringe. The flow rate of the solvent is a function of the pressure and the size of the tip orifice. While the dispense rate scales roughly linearly with the pressure, it is an exponential function of the tip orifice.
 
Observed dispense rates of PGMEA (uncertainty from measurements ~0.1 ml/s) for different tip sizes:
*'''Red (0.010"):'''
**0.2 ml/s @ 0.1 bar
**0.25 ml/s @ 0.2 bar
*'''Purple (0.020"):'''
**0.3 ml/s @ 0.1 bar
**0.65 ml/s @ 0.2 bar
*'''Pink (0.024"):'''
**0.5? ml/s @ 0.1 bar (not verified)
*'''Grey (0.047"):'''
**~2.5 ml/s @ 0.1 bar
 
=Recipes=
Auxiliary recipes, and template recipes. For each case a list of the steps/parameters in the respective recipe.
 
Process recipes developed by Nanolab are listed under Process results.
 
==Auxiliary recipes==
*'''1 DCH Centering test'''
5s @ 100rpm; 5s @ 250rpm; 5s @ 500rpm.
*'''1 DCH Chuck cleaning'''
10s @ 100rpm; 1s @ 0rpm; 10s @ -30rpm; 20s @ 1500rpm.
*'''1 DCH Gyrset cleaning'''
Gyrset down; 10s @ 100rpm; 1s @ 0rpm; 10s @ -30rpm; 20s @ 1500rpm; Gyrset up.
*'''1 DCH predispense'''
0.2s dispense at cup (arm position 0mm).
 
==Manual dispense templates==
*'''1 TMPLT man disp'''
Spin-off; deceleration.
*'''1 TMPLT man disp spread'''
Spread step; spin-off; deceleration.
*'''1 TMPLT man disp Gyrset'''
Gyrset down; spin-off; deceleration; Gyrset up.
*'''1 TMPLT man disp Gyrset sprd'''
Gyrset down; spread step; spin-off; deceleration; Gyrset up.
 
==Automatic dispense templates==
*'''1 TMPLT aut disp SU8'''
Dispense; SU-8 string breaking; spread step; spin-off; deceleration.
*'''1 TMPLT aut disp SU8 Gyrset'''
Dispense; SU-8 string breaking; Gyrset down; spread step; spin-off; deceleration; Gyrset up.
*'''1 TMPLT aut disp'''
Dispense; spin-off; deceleration.
*'''1 TMPLT aut disp spread'''
Dispense; spread step; spin-off; deceleration.
*'''1 TMPLT aut disp Gyrset'''
Dispense; Gyrset down; spin-off; deceleration; Gyrset up.
*'''1 TMPLT aut disp Gyrset sprd'''
Dispense; Gyrset down; spread step; spin-off; deceleration; Gyrset up.
 
=Processing results=
 
==SU-8 2075==
[[Image:RCD8 SU-8 2075.jpg|300x300px|thumb|right|Spin curve for SU-8 2075]]
[[Image:RCD8 SU-8 2075 Gyrset.jpg|300x300px|thumb|right|Spin curve for SU-8 2075 using Gyrset]]
Spin coating of SU-8 2075 on Spin Coater: RCD8 using automatic dispense consists of three process steps: static dispense, spread, and spin-off. In the static dispense step the media arm is moved to the center of the wafer, and resist is dispensed for 7s, yielding a volume of 3.5ml at 2.0 bar. After the dispense, the media arm is moved up and down in a series of steps designed to break the string of resist between the syringe and the wafer. In the spread step the wafer is accelerated to 700rpm at 50rpm/s, and spun for 25s. In the spin-off step the wafer is accelerated at 500rpm/s to the spin-off speed, spun for 30s, then decelerated at 1000rpm/s.
<br>In the Gyrset version, the Gyrset is closed after the dispense step, and opened after the spin-off step.
 
''Recipe names, process parameters, and test results:''
*'''1 DCH SU8 aut disp 100um'''
Spin-off: 30 s at 2100 rpm.
 
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"
|-
|-style="background:silver; color:black"
!Substrate
!Thickness
!Uniformity (+/-)
!Test date
!Tester initials
!Comments
|-
|-style="background:WhiteSmoke; color:black"
|Silicon with native oxide
|100 µm
|3.5%
|14/4 2015
|taran
|5 points on one wafer, exclusion zone 15mm
|}
 
 
*'''1 DCH SU8 aut dsp Grst 100um'''
Spin-off: 30 s at 2000 rpm.
 
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"
|-
|-style="background:silver; color:black"
!Substrate
!Thickness
!Uniformity (+/-)
!Test date
!Tester initials
!Comments
|-
|-style="background:WhiteSmoke; color:black"
|Silicon with native oxide
|99 µm
|3.0%
|15/4 2013
|taran
|5 points on one wafer, exclusion zone 15mm
|}
 
<br clear="all" />
 
==AZ 4562==
[[Image:RCD8 AZ 4562.jpg|300x300px|thumb|right|Spin curve for AZ 4562]]
Spin coating of AZ 4562 on Spin Coater: RCD8 using manual dispense is a very simple process. The wafer is accelerated at 1000rpm/s to the spin-off speed, spun for 30s, then decelerated at 1000rpm/s.
 
''Recipe names, process parameters, and test results:''
*'''1 DCH 4562 man disp 10um'''
Spin-off: 30 s at 2000 rpm.
 
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"
|-
|-style="background:silver; color:black"
!Substrate
!Thickness
!Uniformity (+/-)
!Test date
!Tester initials
!Comments
|-
|-style="background:WhiteSmoke; color:black"
|Silicon with native oxide
|9.92 µm
|2.9%
|29/4 2015
|taran
|9 points on one wafer, exclusion zone 5mm <br> Non-vacuum chuck
|}
 
<br clear="all" />
 
==AZ 5214E==
[[Image:RCD8 AZ 5214E.jpg|300x300px|thumb|right|Spin curve for AZ 5214E]]
Spin coating of AZ 5214E on Spin Coater: RCD8 using manual dispense is a very simple process. The wafer is accelerated at 1000rpm/s to the spin-off speed, spun for 30s, then decelerated at 1000rpm/s.
 
''Recipe names, process parameters, and test results:''
 
*'''1 DCH 5214E man disp 2.2um'''
Spin-off: 30 s at 2100 rpm.
 
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"
|-
|-style="background:silver; color:black"
!Substrate
!Thickness
!Uniformity (+/-)
!Test date
!Tester initials
!Comments
|-
|-style="background:WhiteSmoke; color:black"
|Silicon with native oxide
|2.19 µm
|0.4%
|22/4 2013
|taran
|9 points on one wafer, exclusion zone 5mm
|}
 
<br clear="all" />


The wafer is first centered on the spindle chuck and held in place by vacuum. If static dispense is specified in the process, the spindle remains static during the ensuing resist dispense. In the case of dynamic dispense, the spindle is accelerated to a low spin speed before the resist is dispensed. Using too high spin speed during dispense can cause surface wetting issues, while a too low spin speed causes the resist to flow onto the backside of the wafer. The resist is dispensed through the dispense arm, positioned over the center of the wafer. The resist pump administers a fixed volume of resist (4 ml), but multiple dispenses may be used. After dispense, a short spin at low spin speed may be used in order to spread the resist over the wafer surface before spin-off.  
==AZ MiR 701==
[[Image:RCD8 AZ MiR 701.jpg|300x300px|thumb|right|Spin curve for AZ MiR 701 (29cps)]]
Spin coating of AZ MiR 701 (29cps) on Spin Coater: RCD8 using manual dispense is a very simple process. The wafer is accelerated at 1000rpm/s to the spin-off speed, spun for 30s, then decelerated at 1000rpm/s.


The spin-off cycle determines the thickness of the resist coating. The thickness is primarily a function of the spin-off speed and the spin-off time, both following an inverse power-law (y=k*x^-a). The acceleration to the spin-off speed also influences the thickness, but the effect is dependent on previous steps. The spin-off is usually a simple spin at one speed, but it may be comprised of several steps at different spin speeds. After spin-off, the wafer is decelerated.
''Recipe names, process parameters, and test results:''
*'''1 DCH MiR 701 man disp 2um''' <sup>1)</sup>
Spin-off: 30 s at 2350 rpm.


During spin coating, resist builds up at the edge of the wafer due to the change in surface tension at the edge. This phenomenon is called an edge-bead. Dependent on spin coating parameters, the coating may be several times thicker at the edge than in the central area. In a subsequent hard contact exposure step, this edge-bead induces an undesired proximity gap which reduces the lateral resolution, and may even cause the wafer to stick to the mask. In an edge-bead removal step, solvent administered through a nozzle positioned at the edge of the wafer while spinning at low or medium spin speed dissolves the resist and washes it away. After the removal, a short spin at medium spin speed dries the wafer before the soft bake. Dependent on the viscosity (solvent content) of the resist at the point of edge-bead removal, this drying spin may cause the resist to re-flow and create a secondary edge-bead. In some cases, it may be necessary to (partially) soft bake the resist before edge-bead removal.
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"
|-
|-style="background:silver; color:black"
!Substrate
!Thickness
!Uniformity (+/-)
!Test date
!Tester initials
!Comments
|-
|-style="background:WhiteSmoke; color:black"
|Silicon with native oxide
|2.00 µm
|1.8%
|29/4 2015
|taran
|9 points on one wafer, exclusion zone 5mm <br> Non-vacuum chuck
|}


Dependent on the spin speeds used in the various steps of the spin coating, resist may creep over the edge of the wafer and onto the backside. Also, some resists tend to leave fine strings of resist protruding from the edge of the wafer, or folded onto the backside, an effect sometimes referred to as "cotton candy". This resist will contaminate the soft bake hotplate, and thus subsequent wafers with resist. In a backside rinse step, solvent administered through a nozzle to the backside of the wafer while spinning at low or medium spin speed dissolves the resist and washes it away. After the rinse, a short spin at medium spin speed dries the wafer before the soft bake. During the backside rinse solvent inevitably creeps onto the front side of the wafer. This effect may be used to dissolve and subsequently remove an edge-bead, but it may also leave the rim of the wafer exposed. As an alternative to backside rinse, a wafer which is left dirty on the backside by the spin coat process may be soft baked in proximity in order to protect the hotplate from contamination. This leaves front side coating intact, but also leaves the backside dirty.
<sup>1)</sup> Not implemented yet.
<br clear="all" />


=Automatic dispense=
==AZ nLOF 2020==
[[Image:RCD8 AZ nLOF 2020.jpg|300x300px|thumb|right|Spin curve for AZ nLOF 2020]]
Spin coating of AZ nLOF 2020 on Spin Coater: RCD8 using manual dispense is a very simple process. The wafer is accelerated at 1000rpm/s to the spin-off speed, spun for 30s, then decelerated at 1000rpm/s.
 
''Recipe names, process parameters, and test results:''
*'''1 DCH nLOF 2020 man disp 2.3um''' <sup>1)</sup>
Spin-off: 30 s at 2500 rpm.
 
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"
|-
|-style="background:silver; color:black"
!Substrate
!Thickness
!Uniformity (+/-)
!Test date
!Tester initials
!Comments
|-
|-style="background:WhiteSmoke; color:black"
|Silicon with native oxide
|2.30 µm
|1.7%
|29/4-2015
|taran
|9 points on one wafer, exclusion zone 5mm <br> Non-vacuum chuck
|}
 
<sup>1)</sup> Not implemented yet.
<br clear="all" />

Revision as of 07:53, 27 October 2023

This section, including all images and pictures, is created by DTU Nanolab staff unless otherwise stated.

Feedback to this page: click here


Spin coating

Spin coating on Spin Coater: RCD8 consists of a selection of the following steps:

  1. Optional: Acceleration to a low spin speed if dynamic dispense is used
  2. Resist dispense
  3. Optional: Closing the Gyrset (if used)
  4. Optional: Resist spreading at low spin speed
  5. Spin-off
  6. Deceleration
  7. Opening Gyrset


The wafer is first centered on the chuck and held in place by vacuum (or pins in the case of the non-vacuum chuck). If static dispense is used, the spindle remains static during the ensuing resist dispense. In the case of dynamic dispense, the spindle is accelerated to a low spin speed before the resist is dispensed. Using too high spin speed during dispense can cause surface wetting issues, while a too low spin speed causes the resist to flow onto the backside of the wafer. The resist may be dispensed manually, or automatically using the syringe dispense system on the media arm. After dispense, a short spin at low spin speed may be used in order to spread the resist over the wafer surface before spin-off.

The spin-off cycle determines the thickness of the resist coating. The thickness is primarily a function of the spin-off speed and the spin-off time, both following an inverse power-law. The acceleration to the spin-off speed also influences the thickness, but the effect is dependent on previous steps. The spin-off is usually a simple spin at one speed, but it may be comprised of several steps at different spin speeds. After spin-off, the wafer is decelerated.

Automatic dispense

Automatic dispense on the Spin Coater: RCD8 is done using a Nordson EFD Performus VII pressurised cartridge dispense system. The syringe containing the resist is mounted on the media arm, and the resist is dispensed using a nitrogen pressure supplied by the control box. The dispense rate is controlled by the nitrogen pressure, while the dispense time, and thus the volume, is set in the recipe. The dispensed volume may be estimated by measuring the distance the resist level is displaced during a dispense, and calculating the corresponding volume using the diameter of the syringe (23 mm). A displacement of 10 mm corresponds to a dispensed volume of 4 mL.

Observed dispense rates (uncertainty from measurements ~0.1 ml/s):

  • SU-8 2075:
    • 0.2 ml/s @ 1.0 bar
    • 0.5 ml/s @ 2.0 bar
    • 0.7 ml/s @ 3.0 bar
  • SU-8 2035:
    • 0.5 ml/s @ 1.0 bar
  • SU-8 2010:
    • 1.1 ml/s @ 0.1 bar
  • KMPR 1025:
    • 0.4 ml/s @ 0.5 bar
    • 0.7 ml/s @ 1.0 bar
  • AZ 5214E:
    • 1.2 ml/s @ 0.1 bar
    • 2.4 ml/s @ 0.18 bar

Edge bead removal

The automatic dispense system may also be used to administer solvent at the edge of the wafer after spin coating in order to remove the edge bead. Edge bead removal, or EBR, is usually done using PGMEA. Due to the low viscosity of the solvent, and the relatively high pressure of the EFD control box, it is necessary to use at tip at the end of the syringe. The flow rate of the solvent is a function of the pressure and the size of the tip orifice. While the dispense rate scales roughly linearly with the pressure, it is an exponential function of the tip orifice.

Observed dispense rates of PGMEA (uncertainty from measurements ~0.1 ml/s) for different tip sizes:

  • Red (0.010"):
    • 0.2 ml/s @ 0.1 bar
    • 0.25 ml/s @ 0.2 bar
  • Purple (0.020"):
    • 0.3 ml/s @ 0.1 bar
    • 0.65 ml/s @ 0.2 bar
  • Pink (0.024"):
    • 0.5? ml/s @ 0.1 bar (not verified)
  • Grey (0.047"):
    • ~2.5 ml/s @ 0.1 bar

Recipes

Auxiliary recipes, and template recipes. For each case a list of the steps/parameters in the respective recipe.

Process recipes developed by Nanolab are listed under Process results.

Auxiliary recipes

  • 1 DCH Centering test

5s @ 100rpm; 5s @ 250rpm; 5s @ 500rpm.

  • 1 DCH Chuck cleaning

10s @ 100rpm; 1s @ 0rpm; 10s @ -30rpm; 20s @ 1500rpm.

  • 1 DCH Gyrset cleaning

Gyrset down; 10s @ 100rpm; 1s @ 0rpm; 10s @ -30rpm; 20s @ 1500rpm; Gyrset up.

  • 1 DCH predispense

0.2s dispense at cup (arm position 0mm).

Manual dispense templates

  • 1 TMPLT man disp

Spin-off; deceleration.

  • 1 TMPLT man disp spread

Spread step; spin-off; deceleration.

  • 1 TMPLT man disp Gyrset

Gyrset down; spin-off; deceleration; Gyrset up.

  • 1 TMPLT man disp Gyrset sprd

Gyrset down; spread step; spin-off; deceleration; Gyrset up.

Automatic dispense templates

  • 1 TMPLT aut disp SU8

Dispense; SU-8 string breaking; spread step; spin-off; deceleration.

  • 1 TMPLT aut disp SU8 Gyrset

Dispense; SU-8 string breaking; Gyrset down; spread step; spin-off; deceleration; Gyrset up.

  • 1 TMPLT aut disp

Dispense; spin-off; deceleration.

  • 1 TMPLT aut disp spread

Dispense; spread step; spin-off; deceleration.

  • 1 TMPLT aut disp Gyrset

Dispense; Gyrset down; spin-off; deceleration; Gyrset up.

  • 1 TMPLT aut disp Gyrset sprd

Dispense; Gyrset down; spread step; spin-off; deceleration; Gyrset up.

Processing results

SU-8 2075

Spin curve for SU-8 2075
Spin curve for SU-8 2075 using Gyrset

Spin coating of SU-8 2075 on Spin Coater: RCD8 using automatic dispense consists of three process steps: static dispense, spread, and spin-off. In the static dispense step the media arm is moved to the center of the wafer, and resist is dispensed for 7s, yielding a volume of 3.5ml at 2.0 bar. After the dispense, the media arm is moved up and down in a series of steps designed to break the string of resist between the syringe and the wafer. In the spread step the wafer is accelerated to 700rpm at 50rpm/s, and spun for 25s. In the spin-off step the wafer is accelerated at 500rpm/s to the spin-off speed, spun for 30s, then decelerated at 1000rpm/s.
In the Gyrset version, the Gyrset is closed after the dispense step, and opened after the spin-off step.

Recipe names, process parameters, and test results:

  • 1 DCH SU8 aut disp 100um

Spin-off: 30 s at 2100 rpm.

Substrate Thickness Uniformity (+/-) Test date Tester initials Comments
Silicon with native oxide 100 µm 3.5% 14/4 2015 taran 5 points on one wafer, exclusion zone 15mm


  • 1 DCH SU8 aut dsp Grst 100um

Spin-off: 30 s at 2000 rpm.

Substrate Thickness Uniformity (+/-) Test date Tester initials Comments
Silicon with native oxide 99 µm 3.0% 15/4 2013 taran 5 points on one wafer, exclusion zone 15mm


AZ 4562

Spin curve for AZ 4562

Spin coating of AZ 4562 on Spin Coater: RCD8 using manual dispense is a very simple process. The wafer is accelerated at 1000rpm/s to the spin-off speed, spun for 30s, then decelerated at 1000rpm/s.

Recipe names, process parameters, and test results:

  • 1 DCH 4562 man disp 10um

Spin-off: 30 s at 2000 rpm.

Substrate Thickness Uniformity (+/-) Test date Tester initials Comments
Silicon with native oxide 9.92 µm 2.9% 29/4 2015 taran 9 points on one wafer, exclusion zone 5mm
Non-vacuum chuck


AZ 5214E

Spin curve for AZ 5214E

Spin coating of AZ 5214E on Spin Coater: RCD8 using manual dispense is a very simple process. The wafer is accelerated at 1000rpm/s to the spin-off speed, spun for 30s, then decelerated at 1000rpm/s.

Recipe names, process parameters, and test results:

  • 1 DCH 5214E man disp 2.2um

Spin-off: 30 s at 2100 rpm.

Substrate Thickness Uniformity (+/-) Test date Tester initials Comments
Silicon with native oxide 2.19 µm 0.4% 22/4 2013 taran 9 points on one wafer, exclusion zone 5mm


AZ MiR 701

Spin curve for AZ MiR 701 (29cps)

Spin coating of AZ MiR 701 (29cps) on Spin Coater: RCD8 using manual dispense is a very simple process. The wafer is accelerated at 1000rpm/s to the spin-off speed, spun for 30s, then decelerated at 1000rpm/s.

Recipe names, process parameters, and test results:

  • 1 DCH MiR 701 man disp 2um 1)

Spin-off: 30 s at 2350 rpm.

Substrate Thickness Uniformity (+/-) Test date Tester initials Comments
Silicon with native oxide 2.00 µm 1.8% 29/4 2015 taran 9 points on one wafer, exclusion zone 5mm
Non-vacuum chuck

1) Not implemented yet.

AZ nLOF 2020

Spin curve for AZ nLOF 2020

Spin coating of AZ nLOF 2020 on Spin Coater: RCD8 using manual dispense is a very simple process. The wafer is accelerated at 1000rpm/s to the spin-off speed, spun for 30s, then decelerated at 1000rpm/s.

Recipe names, process parameters, and test results:

  • 1 DCH nLOF 2020 man disp 2.3um 1)

Spin-off: 30 s at 2500 rpm.

Substrate Thickness Uniformity (+/-) Test date Tester initials Comments
Silicon with native oxide 2.30 µm 1.7% 29/4-2015 taran 9 points on one wafer, exclusion zone 5mm
Non-vacuum chuck

1) Not implemented yet.