Recipes and results - C4F8 / H2 tests

*Unless otherwise stated, all content in this section was done by Maria Farinha@DTU Nanolab, April 2023

Recipe Recipe parameters Process time Date SEM picture Etch rate in SiO2 Etch rate in resist
(AZ5214E inverse)
Selectivity
(SiO2:resist)
SiO2_ICP C4F8= 10 sccm
H2= 28 sccm
Coil= 1000W
Platen= 100W
Press= 2.5mTorr
Temp= 20°C
04:00 min 04/09/2023 211,9 nm/min
+/- 14.6%
153,4 nm/min
+/- 16.7%
1.4
SiO2_ICP C4F8= 10 sccm
H2= 28 sccm
Coil= 800W
Platen= 15W
Press= 2.5mTorr
Temp= 20°C
04:00 min 22/09/2023 134,7 nm/min
+/- 20.8%
145,7 nm/min
+/- 25.1%
0.92