Jump to content

Specific Process Knowledge/Lithography/Baking

From LabAdviser
Revision as of 12:18, 31 July 2026 by Thes (talk | contribs)
(diff) ← Older revision | Latest revision (diff) | Newer revision → (diff)

The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.

Feedback to this page: click here

Comparing baking methods

Spray coater hotplate SU-8 hotplates
(1 & 2 + 3 & 4)
Small benchtop hotplates Gamma hotplates Oven: 110C - 250C Oven 250C
Purpose

Adjustable temperature, contact bake

  • Soft bake
  • PEB
  • Hard bake

Programmable, ramped contact bake

  • Soft bake of SU-8
  • PEB of SU-8

Hotplate: 90-110C:
Programmable, contact bake

  • Soft bake
  • PEB


Labspin hotplates:
Adjustable temperature, contact bake

  • Soft bake
  • PEB
  • Hard bake

Recipe dependent temperature, contact or proximity bake

  • Soft bake
  • PEB
  • Hard bake

Manual convection bake

  • Hard bake
  • Post-exposure bake

Manual convection bake

  • Dehydration
  • NO resist!
Temperature

Maximum 180°C

Temperature with top-plate: Actual surface temperature = 0.9 * display value

Maximum 180°C

Hotplate: 90-110C:

  • Maximum 120°C
  • Return to 90°C after use


Labspin hotplates:

  • Maximum temperature is hotplate dependent
  • Temperature with top-plate: Actual surface temperature = 0.9 * display value

Fixed at various recipe dependent temperatures

110 - 250°C

Return to 110°C after use

Fixed at 250°C

Substrate size
  • Pieces
  • 50 mm wafer
  • 100 mm wafer
  • 150 mm wafer
  • 200 mm wafer
  • pieces
  • 50 mm wafers
  • 100 mm wafers
  • 150 mm wafer
  • 200 mm wafer
  • pieces (only Labspin hotplates)
  • 50 mm wafers
  • 100 mm wafers
  • 150 mm wafer
  • 200 mm wafer
  • 100 mm wafers
  • 150 mm wafers
  • 100 mm wafers
  • 150 mm wafers
  • 100 mm wafers
  • 150 mm wafers
Allowed materials

All substrates

Film or pattern of all types

Silicon, glass, and polymer substrates

Film or pattern of all types except type IV

Hotplate dependent.

(All substrates and film or pattern of all types, unless otherwise noted on the hotplate)

Tool dependent. Typically Silicon, III-V, and glass substrates.

Silicon, glass, and high Tg polymer substrates

Film or pattern of all types

Silicon, glass, and high Tg polymer substrates

Film or pattern of all types except resist

Restrictions
(Not allowed)
III-V, copper, steel substrates

Pb, Te films

Hotplate dependent. Any restrictions will be noted on the hotplate.

Low Tg polymer, copper, steel substrates.

Pb, Te films.

III-V, low Tg polymer, copper, steel substrates III-V, low Tg polymer, copper, steel substrates

Resist is not allowed

QC
- requires login

https://labmanager.dtu.dk/view_binary.php?type=data&mach=293

Hotplate 1:
https://labmanager.dtu.dk/view_binary.php?type=data&mach=122

Hotplate 2:
https://labmanager.dtu.dk/view_binary.php?type=data&mach=124


Hotplate: 90-110C:
https://labmanager.dtu.dk/view_binary.php?type=data&mach=336

Spin coater: Labspin 02:
https://labmanager.dtu.dk/view_binary.php?type=data&mach=362

Spin coater: Labspin 03:
https://labmanager.dtu.dk/view_binary.php?type=data&mach=387

Spincoater: Gamma ebeam & UV:
https://labmanager.dtu.dk/view_binary.php?type=data&mach=417

Spincoater: Gamma UV:
https://labmanager.dtu.dk/view_binary.php?type=data&mach=359

Developer: TMAH UV-lithography:
https://labmanager.dtu.dk/view_binary.php?type=data&mach=329

Spincoater: Süss stepper:
https://labmanager.dtu.dk/view_binary.php?type=data&mach=279

Developer: Stepper:
https://labmanager.dtu.dk/view_binary.php?type=data&mach=328




Hotplates

Hotplate: 90-110C

 
Hotplate: 90-110C located in C-1

Hotplate: 90-110C is used for baking of 2" - 6" wafers. Do not exceed 120°C.


The user manual, and contact information can be found in LabManager:

Hotplate: 90-110C - requires login


SU-8 hotplates

 
Hotplate 1 (SU8) and Hotplate 2 (SU8) (the old set-up in C-1)

We have four hotplates dedicated to baking of SU-8.
Hotplate 1 (SU8) and Hotplate 2 (SU8) are located in cleanroom E-4.
Hotplate 3 (SU8) and Hotplate 4 (SU8) are located in PolyFabLab in building 347.

Users can control the ramp-time, the baking temperature, and the baking time.
The hotplates are temperature limited to 180°C.


The user manual, and contact information can be found in LabManager:

Hotplate 1 (SU8) - requires login

Hotplate 2 (SU8) - requires login

Hotplate 3 (SU8) - requires login

Hotplate 4 (SU8) - requires login

Small benchtop hotplates

Model: Präzitherm PZ 28-2.

Contact bake only. Maximum temperature is hotplate dependent.

Most of these hotplates have been fitted with a top-plate in order to protect the original hotplate surface. With the top-plate, the set point of the controller must be adjusted in order to achieve the correct temperature during the bake:

Actual surface temperature = 0.9 * display value


Gamma hotplates

 
Hotplate modules in Spin Coater: Gamma UV.

Hotplate temperatures are recipe dependent.

Information about the Süss MicroTec Gamma tools can be found in labadviser:


Ovens

Oven: 110C - 250C

 
Oven: 110C - 250C situated in C-1

Variable temperature convection oven mostly used for baking of wafers as a hard baking step after development of photoresist.

The set-point can be varied, but should always be returned to 110°C after use.


The user manual, and contact information can be found in LabManager:

Oven: 110C - 250C - requires login

Oven 250C

 
Oven 250C for pretreatment in Cx-1

The oven is typically used for dehydration pretreatment, of Si and glass substrates, to promote the resist adhesion. We recommend placing the wafers in a metal carrier in the oven for at least for 4 hours, or overnight, and spin coat resist on them as soon as possible after removing them from the oven.


The user manual, and contact information can be found in LabManager:

Oven 250C - requires login