Process runs
Date Substrate Information Process Information SEM Images
Wafer info Mask Material/ Exposed area Tool / Operator Conditioning Recipe Wafer ID Comments
3/12-2014 1/4 6" Wafer with 210 nm oxide and 1800 nm polysilicon CB on oxide carrier standard stepper mask (50 nm barc + 320 nm krf) Si / 50+ % Pegasus/jmli 10 minute TDESC clean + 45 sec barc etch nanolab/jml/showerhead/Cpoly2, 20 cycles or 2:08 minutes S004729 New showerhead

File:S004729-01.jpg File:S004729-02.jpg File:S004729-03.jpg