The nano1.21 recipe

Recipe nano1.21
Recipe Gas C4F8 75 sccm, SF6 38 sccm
Pressure 4 mTorr, Strike 3 secs @ 15 mTorr
Power 800 W CP, 50 W PP
Temperature -10 degs
Hardware 100 mm Spacers
Time 120 secs
Conditions Run ID 1925
Conditioning Sequence: Oxygen clean, MU tests, processes, no oxygen between runs
Mask nm zep etched down to 6dgh4 nm