Sputter technique using IBE/IBSD Ionfab300
|
Sputter-system Metal-Oxide(PC1)
|
Sputter-System(Lesker)
|
ALD Picosun 200
|
| Generel description
|
- TiO2 created from a Ti sputter target. By adding oxygen during the deposition TiO2 is created.
|
- Reactive DC sputtering of Ti target in Ar/O2 plasma
- (Reactive) RF sputtering of TiO2 target
- Reactive pulsed DC sputtering of Ti target in Ar/O2 plasma
- Reactive HIPIMS (high-power impulse magnetron sputtering of Ti target in Ar/O2
|
- Reactive DC sputtering of Ti target in Ar/O2 (10% O2) plasma
- RF sputtering of TiO2 target
|
- ALD (atomic layer deposition) of TiO2
|
| Stoichiometry
|
- Can probably be varied (sputter target: Ti, O2 added during deposition)
|
|
|
- Temperature dependent - Anatase or amorphous TiO2
|
| Film Thickness
|
|
|
|
|
| Deposition rate
|
- 3.0-3.5 nm/min (reactive sputtering)
|
- not yet known, probably faster than Sputter-System(Lesker)
|
- 3-5 nm/min (RF sputtering)
- 0.3 - 0.5 nm/min
|
- 0.06 nm/min - 0.40 nm/min (very recipe and temperature dependent)
|
| Step coverage
|
|
|
|
- Very good. Covers sample everywhere (but long purge time needed for very high aspect ratio structures)
|
| Process Temperature
|
- Expected to be below 100 °C
|
|
|
- 120 °C - 150 °C: Amorphous TiO2
- 300 °C - 350 °C: Anatase TiO2
|
| More info on TiO2
|
|
|
|
ALD1:
ALD2:
|
| Substrate size
|
- 1 50mm wafer
- 1 100mm wafer
- 1 150mm wafer
- 1 200mm wafer
- Smaller pieces can be mounted with capton tape
|
- many small samples
- Up to 10x 100 mm or 150 mm wafers
|
- several small samples
- several 50 mm wafers (Ø150mm carrier)
- 1x 100 mm wafers
- 1x 150 mm wafers
|
ALD1:
- 1-5 100 mm wafers
- 1-5 150 mm wafers
- 1 200 mm wafer
- Several smaller samples
ALD2:
- 1 100 mm wafer
- 1 150 mm wafer
- 1 200 mm wafer
- Several smaller samples
|
| Allowed materials
|
- Almost any materials
- not Pb and very poisonous materials
|
- Almost any materials
- Pb and poisonous materials only after special agreement
|
|
- Silicon
- Silicon oxide, silicon nitride
- Quartz/fused silica
- Metals - Use a dedicated carrier wafer
- III-V materials - Use dedicated carrier wafer
- Polymers - Depending on the melting point/deposition temperature, use dedicated carrier wafer. Ask for permission
|