Jump to content

Specific Process Knowledge/Etch/Wet Aluminium Etch

From LabAdviser

THIS PAGE IS UNDER CONSTRUCTION

Feedback to this page: click here

Wet ething of aluminium can be done using many different acids and bases. Using dilute phosphoric acid gives reasonably good control and compatibility with photoresists. Etching with dilute phosphoric acid is suitable for etching pure aluminium. If the aluminium is alloyed with other metals, other etchants may be better suited. Previously, aluminium with 1,5% silicon was used at DTU Danchip. This alloy is no longer in use at DTU Danchip but a suitable etchant (PES 77-19-04) for this alloy is included below.

Wet Aluminium Etch

 
Aluminium Etch bath located in left side of Wet bench 05 in cleanroom D-3

Wet etching of aluminium is done with two different solutions:

  1. H2O:H3PO4 1:2 at 50 oC
  2. Pre-mixed etch solution: PES 77-19-04 at 20 oC

Both solutions are used in the Aluminium etch bath shown to the right. It must be written on which one is in. Solution no. 1 is the most used solution for etching aluminium. Solution no. 2 is primarily for etching aluminium mixed with a small percentage of silicon.

The user manual and contact information can be found in LabManager:

Al-etch info page in LabManager

Comparing the two solutions

Aluminium Etch 1 Aluminium Etch 2
General description Etch of pure aluminium Etch of aluminium + 1.5% Si
Link to KBA

see KBA here

see KBA here

Chemical solution H2O:H3PO4 1:2 PES 77-19-04

77 vol% H3PO4 85%

19 vol% CH3COOH 100%

4 vol% HNO3 70%

Process temperature! 50 oC 20 oC
Possible masking materials! Photoresist (1.5 µm AZ5214E) Photoresist (1.5 µm AZ5214E)
Etch rate ~100 nm/min (Pure Al) ~60 nm/min
Batch size! 1-25 wafers at a time 1-25 wafer at a time
Size of substrate 4" wafers 4" wafers
Allowed materials
  • Aluminium
  • Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride
  • Photoresist
  • E-beam resist
  • Aluminium
  • Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride
  • Photoresist
  • E-beam resist