Specific Process Knowledge/Thin film deposition/Deposition of Vanadium Silicide/V3Si RF-DC Co-Sputtering in Cluster Lesker PC3
This page is written by Evgeniy Shkondin @ DTU Nanolab if nothing else is stated.
All images and data on this page belong to DTU Nanolab.
The exploratory deposition and characterization described below were performed in 2025.
Exploratory V-Si RF-DC co-sputtering in Cluster Lesker PC3
This page documents an early, non-systematic attempt to deposit vanadium silicide by simultaneous RF sputtering of a 4-inch Si target and DC sputtering of a 3-inch V target in the Cluster Lesker PC3 chamber. Two otherwise nominally identical depositions were compared: one without RF substrate bias and one with 30 W RF substrate bias.
The experiment gave a striking result. In the measured 30–80° GiXRD range, the unbiased sample showed only reflections assigned to cubic A15 V3Si, whereas the sample deposited with 30 W RF substrate bias showed only reflections assigned to hexagonal C40 VSi2. The two samples also had very different surface morphologies and sheet resistances.
This PC3 experiment is separate from the later, systematic V3Si process-development study performed in PC1.
Substrate and deposition conditions
- Substrate: 150 mm Si(100) wafer
- Surface preparation: native SiO2 removed by HF immediately before deposition
- Si source: 4-inch Si target, RF sputtering
- V source: 3-inch V target, DC sputtering
- Working pressure: 3 mTorr
- Deposition temperature: 600 °C
- Deposition time: 1200 s
- Substrate-bias comparison: no RF bias versus 30 W RF bias
- Recorded DC substrate-bias voltage at 30 W RF bias: 69 V
| Condition | Si target | Si power | Displayed Si voltage | V target | V power | Displayed V voltage | Pressure | RF substrate power | Substrate DC bias | Temperature | Time |
|---|---|---|---|---|---|---|---|---|---|---|---|
| No substrate bias | 4-inch Si | 120 W RF | 100 V | 3-inch V | 100 W DC | 322 V | 3 mTorr | 0 W | Not applied | 600 °C | 1200 s |
| 30 W RF substrate bias | 4-inch Si | 120 W RF | 110 V | 3-inch V | 100 W DC | 309 V | 3 mTorr | 30 W | 69 V | 600 °C | 1200 s |
Although the applied target powers were unchanged, the displayed Si and V discharge voltages changed when the substrate RF bias was enabled. This shows that the plasma impedance/coupling was not identical in the two runs. Consequently, the elemental rates measured in separate calibration depositions should be treated as nominal flux estimates rather than exact in-situ co-deposition rates.
Power calibration and estimated V:Si atomic-arrival ratio
The individual elemental deposition rates measured at 3 mTorr were:
| Element | Target size | Mode | Power | Pressure | Pure-element thickness rate | Density used | Molar mass used |
|---|---|---|---|---|---|---|---|
| Si | 4 inch | RF | 120 W | 3 mTorr | 0.024 nm/s | 2.329 g/cm3 | 28.0855 g/mol |
| V | 3 inch | DC | 100 W | 3 mTorr | 0.0700 nm/s | 6.11 g/cm3 | 50.9415 g/mol |
The thickness-rate ratio was therefore:
This number cannot be compared directly with the 3:1 atomic stoichiometry of V3Si. For an elemental rate calibration, the atomic arrival rate is proportional to:
where is the elemental density, is the pure-element thickness rate, and is the molar mass. The nominal target-derived atomic-arrival ratio is consequently:
Thus, the flux supplied by the two targets was nominally about 80.8 at.% V and 19.2 at.% Si, corresponding to V4.22Si rather than V3Si. The pure-element thickness-rate ratio required for an atomic V:Si ratio of 3 is approximately:
The calibrated target flux was therefore substantially more V-rich than the ideal V3Si value. The formation of V3Si in the unbiased sample cannot be explained by the target flux alone; Si supplied by the oxide-stripped Si wafer must be considered.
Simple target/substrate mass balance
Using the calibrated rates and 1200 s deposition time, and assuming for the moment that all deposited V was retained:
- formation of V3Si requires approximately 11.7 nm of substrate-equivalent Si in addition to the Si supplied by the target;
- the corresponding full-retention V3Si layer thickness is approximately 105 nm using a bulk V3Si density of 5.77 g/cm3;
- the measured no-bias XRR thickness was 94.046 nm, about 89% of this simple mass-balance value.
The agreement is reasonable for separately calibrated rates, compound formation, a simplified XRR model, and a process performed at 600 °C. It supports substrate participation but is not an independent composition measurement.
If all calibrated V instead formed VSi2, the limiting mass balance would require approximately 214 nm of additional substrate-equivalent Si and would produce roughly 244 nm of VSi2 using a density of 4.42 g/cm3. These are not measured values for the biased sample. They illustrate that formation of VSi2 throughout the deposited material would require extensive Si uptake from the wafer, a change in retained V flux, or both.
Characterization methods
X-ray reflectivity (XRR)
XRR measurements were performed using a Rigaku SmartLab X-ray diffractometer. The Cu X-ray tube was operated at 40 kV and 30 mA. The incident optics included an IPS (incident parallel-slit) adapter with a 5° Soller slit. The slit configuration was IS = 0.05 mm, RS1 = 0.05 mm and RS2 = 0.075 mm. The programmed scan used a step size of 0.01° and a counting time of 2 s per point. The MATLAB analysis reads the actual exported angular coordinates and does not assume a fixed data interval.
Grazing-incidence X-ray diffraction (GiXRD)
GiXRD measurements were performed using the Rigaku SmartLab instrument with a Cu sealed X-ray tube operated at 40 kV and 30 mA. The scans covered 30–80° in 2θ, using a 0.5 mm incident slit, a step size of 0.01° and a scan speed of 2°/min. The incident angle was fixed at relative to the sample surface.
The shallow fixed incidence increases the film contribution relative to a conventional symmetric scan. Phase assignment is based on the observed reflection series. Reported lattice parameters are approximate because the scans were not subjected to a full instrumental-zero/refraction refinement and the sealed-tube spectrum can contain unresolved Cu Kα contributions.
Scanning electron microscopy (SEM)
Plan-view SEM images were recorded at 5.00 kV with the InLens detector. Images were acquired at 200,000× and 300,000× magnification. The original scale bars and acquisition metadata are retained in the TIFF images.
Sheet resistance
Room-temperature sheet resistance was measured for both samples. Resistivity is calculated only for the unbiased sample because only that sample has a defensible XRR thickness.
Results overview
| Condition | Crystalline phase detected by GiXRD | Lattice parameters from GiXRD | XRR thickness | XRR density | XRR roughness | Sheet resistance | Calculated resistivity |
|---|---|---|---|---|---|---|---|
| No substrate bias | V3Si, cubic A15 | Å1 | 94.046 nm | 4.741 g/cm3 | 7.873 nm | 29.34 Ω/sq | 276 µΩ·cm |
| 30 W RF substrate bias (69 V DC bias) | VSi2, hexagonal C40 | Å, Å1 | Not obtained; surface too rough for a defensible fit | Not obtained | Not obtained | 6.64 Ω/sq | Not calculated because thickness is unknown |
1 Values are derived from pseudo-Voigt fits to several assigned GiXRD reflections using Cu Kα1 = 1.540593 Å. They should be regarded as approximate GiXRD lattice parameters, not high-resolution lattice refinements.
Grazing-incidence X-ray diffraction results
-
GiXRD comparison of the two PC3 depositions. The temperature shown in the figure is corrected to 600 °C, even though the original data filenames contain 500C.
Unbiased film: A15 V3Si
The unbiased sample contains the characteristic A15 V3Si reflection series. The main fitted peaks are:
| Reflection | Fitted 2θ | Approximate apparent coherence length2 |
|---|---|---|
| V3Si (200) | 38.03° | 13.0 nm |
| V3Si (210) | 42.70° | 10.8 nm |
| V3Si (211) | 46.99° | 14.4 nm |
| V3Si (320) | 71.95° | 16.8 nm |
| V3Si (321) | 75.00° | 12.5 nm |
The mean cubic lattice parameter obtained from the five reflections is Å. This is slightly larger than the commonly reported room-temperature bulk value of approximately 4.72 Å, but the difference is too small to interpret confidently without a zero-shift/reference correction and a dedicated high-resolution scan.
30 W RF-biased film: C40 VSi2
The biased sample contains the reflection series expected for C40 VSi2. The fitted peaks used for the lattice calculation are:
| Reflection | Fitted 2θ | Comment |
|---|---|---|
| VSi2 (110) | 39.43° | Isolated peak |
| VSi2 (111) | 41.96° | Fitted together with (003) |
| VSi2 (003) | 42.50° | Fitted together with (111) |
| VSi2 (112) | 48.98° | Several C40 reflections are close in this region |
| VSi2 (031) | 73.12° | High-angle constraint |
| VSi2 (032) | 78.32° | High-angle constraint |
A simultaneous least-squares solution of the hexagonal d-spacing relation gives Å and Å, in good agreement with reported C40 VSi2 lattice parameters.
In both samples, “single phase” means that no other crystalline phase was resolved above the detection/background limit within the measured 30–80° range. The scans do not exclude amorphous material, a thin interfacial phase, or a minor crystalline fraction hidden by peak overlap.
2 The coherence lengths are Scherrer estimates based on uncorrected fitted FWHM values. Instrumental broadening, microstrain, texture, peak overlap, and the Cu Kα doublet were not separated. These numbers are therefore approximate coherent-domain sizes and must not be equated directly with SEM surface-feature size.
X-ray reflectivity results
-
XRR comparison and the exported fit for the unbiased sample. The strong damping/absence of useful fringes from the biased sample prevents a reliable thickness fit.
The unbiased sample could be represented by a simplified single vanadium-silicide layer on Si:
- thickness: 94.046 nm;
- fitted density: 4.741 g/cm3;
- fitted layer roughness: 7.873 nm;
- thickness-derived growth rate: 0.0784 nm/s.
The fitted density is about 82% of the 5.77 g/cm3 bulk value used for V3Si. This can reflect porosity/voids, oxidation, model-density/roughness correlation, lateral non-uniformity, or a more complicated interface than the one-layer model. XRR density alone is not a chemical-composition measurement.
The 30 W RF-biased film was too rough for a defensible XRR model. No thickness, density, roughness or resistivity should be quoted from this scan. A cross-sectional measurement is needed.
SEM surface morphology
-
Plan-view SEM comparison at 200,000× and 300,000×. Original scale bars and microscope metadata are preserved in each panel.
Both films are rough and polycrystalline, but the morphologies differ strongly:
- the unbiased V3Si film consists mainly of much finer, densely distributed granular/nodular surface features, with occasional brighter agglomerates;
- the 30 W-biased VSi2 film contains substantially larger faceted plate-like grains, many with visible terraces or banded surface contrast;
- the coarser faceted morphology of the biased sample is consistent with its strongly damped XRR response, but plan-view SEM cannot provide an RMS roughness or film thickness.
Electrical results
The unbiased V3Si sample had a sheet resistance of 29.34 Ω/sq. Combining this value with the XRR thickness gives:
The 30 W-biased VSi2 sample had a much lower sheet resistance of 6.64 Ω/sq, but this does not by itself demonstrate a lower material resistivity or a better film. Sheet resistance depends on both resistivity and thickness. The biased layer may be considerably thicker because of reaction with the Si wafer, may contain an electrically parallel interfacial/unreacted layer, or may simply have a different intrinsic resistivity and connectivity. Until its thickness and cross-sectional structure are measured, only the sheet resistance should be reported.
Interpretation of the bias-induced phase change
The most likely working interpretation is that the oxide-stripped Si substrate was an active reactant and that RF substrate bias changed the early interface reaction sufficiently to select a different silicide phase.
- The targets supplied a V-rich flux. The estimated target-derived atomic ratio was V:Si = 4.22, which is more V-rich than V3Si. Formation of V3Si in the unbiased sample therefore requires some Si uptake from the wafer, but only a modest amount: approximately 11.7 nm of substrate-equivalent Si in the simple full-retention mass balance.
- Bare crystalline Si provides a very large Si reservoir. Earlier V/Si interface studies report that VSi2 is the first silicide phase to nucleate and grow at a single-crystal Si/V interface. More recent V3Si work likewise shows that limiting the available Si favors the V-rich A15 phase, whereas an unrestricted Si supply favors Si-rich silicides.
- The unbiased run may have formed an early V3Si-rich reaction layer. With the V-rich incoming flux, such a layer could kinetically limit further Si transport from the wafer and preserve the A15 phase during the remainder of the 1200 s deposition.
- The 69 V substrate DC bias introduced energetic ion bombardment. Ion bombardment can increase defect generation, surface mobility, atomic mixing and re-sputtering. In this experiment it may have disrupted or delayed formation of the V3Si-rich barrier, enhanced access to substrate Si, and allowed the thermodynamically/kinetically favored Si-rich VSi2 reaction to continue. This is a plausible mechanism, not a direct measurement.
- The bias also changed the plasma state. The Si display changed from 100 to 110 V and the V discharge voltage from 322 to 309 V at fixed applied target powers. The actual V and Si arrival rates may therefore have shifted relative to the separate elemental calibrations. Voltage alone is insufficient to calculate the change in composition.
The data demonstrate that 30 W RF substrate bias is not a small microstructural adjustment for this process. On HF-stripped Si at 600 °C it changes the detected crystalline product from V3Si to VSi2 and produces a much coarser surface morphology.
Limitations
- Only two depositions were compared; there is no bias-power series and no repeatability test.
- The elemental deposition rates were measured separately, not simultaneously during co-sputtering at 600 °C.
- No direct V:Si composition measurement is available.
- GiXRD establishes crystalline phase identity within its detection limits but does not quantify amorphous material or reliable phase fractions.
- The biased sample has no measured thickness; therefore its resistivity and true deposition/reaction rate are unknown.
- Plan-view SEM does not reveal the film/substrate interface or how much Si was consumed.
- The influence of the HF-to-load delay and any regrown interfacial oxide was not isolated.
- Phase-pure A15 diffraction does not by itself prove superconductivity; a temperature-dependent resistance measurement is required.
References
- W. Zhang et al., “Thin-film synthesis of superconductor-on-insulator A15 vanadium silicide,” Scientific Reports 11, 2358 (2021), DOI: 10.1038/s41598-021-82046-1. This work discusses control of Si supply during V3Si formation and provides the V/Si molar-volume calculation used as a cross-check here.
- R. J. Schutz et al., “The formation of vanadium silicides at thin-film interfaces,” Journal of Applied Physics 50, 5773–5781 (1979), DOI: 10.1063/1.326718. This study reports VSi2 as the first silicide phase to nucleate and grow at single-crystal Si/V interfaces.
- M. Bose et al., “In-situ Investigation of the Phase Formation and Superconductivity in V3Si Thin Films at High Temperatures,” arXiv:2412.04159. This work shows that interface/barrier consumption and excessive Si access can drive formation of undesirable Si-rich silicides.
- M. Manzo-Perez et al., “Substrate effects on phase formation and interfacial stability in superconducting vanadium silicide thin films,” Applied Physics Letters 127, 122601 (2025), DOI: 10.1063/5.0291576.