Revision as of 12:42, 16 September 2025 by Pevo (talk | contribs) (Created page with "==Breakdown voltage results for the A3 Phosphorus Drive-in furnace== ===Dry oxidation=== {| border="2" cellspacing="2" cellpadding="5" style="text-align: center;" |- |'''Date''' |'''Oxidation recipe''' |'''Oxide thickness''' |'''Absolute break-down voltage''' |'''Relative break-down voltage''' |- |'''November 2021''' |DRY1050 |118 nm |350x350px|thumb|left |image:2021-11-09_08-27-49_Wafer_A3_DRY1050_118nm_R...")
(diff) ← Older revision | Latest revision (diff) | Newer revision → (diff)

Breakdown voltage results for the A3 Phosphorus Drive-in furnace

Dry oxidation

Date Oxidation recipe Oxide thickness Absolute break-down voltage Relative break-down voltage
November 2021 DRY1050 118 nm
February 2022 DRY1050 113 nm
September 2023 DRY1050 113 nm
November 2023 DRY1100 490 nm
February 2024 DRY1050 115 nm
April 2025 DRY1050 114 nm

Wet oxidation

Date Oxidation recipe Oxide thickness Absolute break-down voltage Relative break-down voltage
November 2021 WET1050 ~320 nm
January 2024 WET1050 ~308 nm