Specific Process Knowledge/Etch/DRIE-Pegasus/nanoetch/nano14
The nano1.4 recipe
Recipe | Gas | C4F8 75 sccm, SF6 38 sccm |
---|---|---|
Pressure | 4 mTorr, Strike 3 secs @ 15 mTorr | |
Power | 800 W CP, 50 W PP | |
Temperature | -20 degs | |
Hardware | 100 mm Spacers | |
Time | 120 secs | |
Conditions | Run ID | 2000 |
Conditioning | Sequence: Oxygen clean, MU tests, processes, no oxygen between runs | |
Mask | 211 nm zep etched down to 77 nm |
-
The 30 nm trenches
-
The 60 nm trenches
-
The 90 nm trenches
-
The 120 nm trenches
-
The 150 nm trenches