Jump to content

Specific Process Knowledge/Lithography/PMMA

From LabAdviser
Revision as of 15:09, 30 October 2015 by Tigre (talk | contribs) (Created page with "{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" width="90%" |- |- |-style="background:Black; color:White" |'''Resist''' |'''Polarity''' |'''Manufacturer...")
(diff) ← Older revision | Latest revision (diff) | Newer revision → (diff)
Resist Polarity Manufacturer Comments Technical reports Spinner Developer Rinse Remover Process flows (in docx-format)
CSAR Positive AllResist Standard positive resist, very similar to ZEP520. Allresist_CSAR62_English.pdf‎,, CSAR_62_Abstract_Allresist.pdf‎ Manual Spinner 1 (Laurell), Spin Coater Labspin XAR-600-546, XAR-600-548, N50, MIBK:IPA IPA AR-600-71, 1165 Remover Process Flow CSAR.docx‎


Spin Curves

The thickness is measured on VASE Ellipsometer using a simple Cauchy model for a transparent polymer on Si. The measurements are performed at one incidence angle (70 degrees) only. 9 points on each 4" wafer has been measured; the standard deviation thus representing the homogeinity of the film on the 4" wafers.

Please be aware that I have experienced a somewhat large thickness deviation (5-8 %) depending on the amount of resist applied to the wafer before spin coating.


Dosepattern has been e-beam exposured and SEM inspected on those wafers marked by silver gray.


AllResist AR-P 6200 (> 2ml per 4" wafer) spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 09-04-2014. Softbake 5 min @ 150 degC.
Spin Speed [rpm] Acceleration [1/s2] Thickness [nm] St Dev
2000 4000 225.98 0.97
3000 4000 194.00 0.6
4000 4000 169.57 0.32
5000 4000 151.47 0.26
6000 4000 142.38 0.41
7000 4000 126.59 0.36


AllResist CSAR (< 2ml per 4" wafer) on Spin Coater: Manual LabSpin A-5, TIGRE, 16-06-2014. Softbake 2 min @ 150 degC.
Spin Speed [rpm] Acceleration [1/s2] Thickness [nm] St Dev
3000 4000 201.61 1.20
4000 4000 173.89 0.64
5000 4000 155.91 0.65


AllResist CSAR 1:1 in anisole (< 2ml per 4" wafer), Spin Coater: Manual LabSpin A-5, TIGRE, 16-06-2014. Softbake 2 min @ 150 degC.
Spin Speed [rpm] Acceleration [1/s2] Thickness [nm] St Dev
2000 4000 83.48 0.49
3000 4000 67.12 0.41
4000 4000 58.64 0.44
5000 4000 53.13 0.39
6000 4000 48.76 0.38