Specific Process Knowledge/Etch/DRIE-Pegasus/nanoetch/nano11
The nano1.1 recipe
Recipe | Gas | C4F8 38 sccm, SF6 52 sccm |
---|---|---|
Pressure | 4 mTorr, Strike 3 secs @ 15 mTorr | |
Power | 600 W CP, 50 W PP | |
Temperature | 10 degs | |
Hardware | 100 mm Spacers | |
Time | 120 secs | |
Conditions | Run ID | 1815 |
Conditioning | Sequence: Oxygen clean, MU tests, processes, no oxygen between runs | |
Mask | 1dfhj10 nm zep etched down to 6dgh4 nm |
-
The 30 nm trenches
-
The 60 nm trenches
-
The 90 nm trenches
-
The 120 nm trenches
-
The 150 nm trenches
Comments
The lower coil power run may still be isotropic-looking either because of a lack of deposition in the process, or because the bias increases as the coil power is decreased, hence the wafer would have received a more phyisically-aggressive process. Lower temp, lower coil + lower platen may be worth a look.