Revision as of 12:44, 13 January 2026
Developer: TMAH Manual 02

Developer: TMAH Manual 02 is a manually operated puddle developer for single wafers or chips. The wafers or chips are loaded manually one by one into the developer, but the developer dispense, puddle time, water rinse, and drying is performed automatically.
The development uses the TMAH based AZ 726 MIF developer (2.38 % TMAH in water with a small amount of wetting agent).
The user manual, user APV, and contact information can be found in LabManager - requires login
Process information
All recipes use the following structure:
- Pressurize the TMAH canister
- Dispense puddle while rotating substrate slowly
- Puddle development with agitation of substrate
- Spin off developer
- Clean substrate and chamber with DI water
- Dry substrate and chamber with nitrogen
Multipuddle recipes repeat steps 2-4 for the given number of puddles.
Process recipes
(Updated 2026-01-12, JEHEM)
- -Rinse-
- 1x015s
- 1x030s
- 1x060s
- 1x120s
- 2x060s
- 5x060s
Agitation
Testing showed that adding agitation to the puddle step gave better uniformity in the development rate over the entire area of the substrate as well as increased development rate.
Tests were performed on under-exposed resist, specifically for showing the difference between the agitation and non-agitation puddle development - the measured results cannot necessarily be transferred directly to a working process, only the vague general behavior of the two process setups; faster/slower development speed and better/worse uniformity across substrate.
| Non-agitation | Agitation | |
|---|---|---|
| Test results |
|
|
| Normalized development rate | 1 | 1.20 |
| Non-uniformity | 21% | 11% |
| Agitation | None | 15 cycles per minute, 20 rpm, 500 rpm/s |
| Substrate | 100 mm SSP silicon | |
| Resist | AZ 5214E | |
| Exposure dose | 50 mJ/cm2 (~50% of normal dose) | |
| Development | Single puddle for 60 seconds | |
| Developer | AZ 726 MIF (2.38% TMAH) | |
-
Development rate for under-exposed resist test
-
Non-uniformity for under-exposed resist test
| Tool purpose |
Development of UV resists:
Development of DUV resists:
|
|---|---|
| Developer | AZ 726 MIF (2.38% TMAH) |
| Development method | Puddle |
| Handling method |
|
| Process temperature | Room temperature |
| Process agitaion | 15 cycles per minute |
| Process rinse | DI water |
| Substrate sizes |
|
| Substrate materials |
|
| Substrate batch size | 1 |