Jump to content

Specific Process Knowledge/Thin film deposition/Electroplating-Ni: Difference between revisions

Reet (talk | contribs)
Mmat (talk | contribs)
mNo edit summary
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:fabricationSupport@Nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Electroplating-Ni click here]'''
'''<p style="color:red;">The Electroplater Technotrans microform.200 has been decomissioned and is no longer available.</p>'''
 
'''Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.'''
 
'''THIS MACHINE HAS BEEN DECOMMISSIONED'''


[[Category: Equipment|Thin film Electroplating Ni]]
[[Category: Equipment|Thin film Electroplating Ni]]
[[Category: Thin Film Deposition|Electroplating Ni]]
[[Category: Thin Film Deposition|Electroplating Ni]]


== Technotrans microform.200 - DECOMMISSIONED==
== Technotrans microform.200==


[[image:Electroplater-D3.jpg|200x200px|right|thumb|Electroplating-Ni positioned in cleanroom D-3]]
[[image:Electroplater-D3.jpg|200x200px|right|thumb|Electroplating-Ni positioned in cleanroom D-3]]