Specific Process Knowledge/Etch/ICP Metal Etcher/Chromium/End point: Difference between revisions
Appearance
| Line 9: | Line 9: | ||
I recorded the end point signal and tried three different stopping times to figure out when to stop the etch. I want to find out how I can use the end point signal to get the best etch result; Etch through - also in the small patterns without too much over etch. | I recorded the end point signal and tried three different stopping times to figure out when to stop the etch. I want to find out how I can use the end point signal to get the best etch result; Etch through - also in the small patterns without too much over etch. | ||
I was looking at trenches with sizes ranging from 200 nm to 2 µm in width. The masking materials was negative DUV resist: NUV 2300-0.5 of approximately 500 nm. | I was looking at trenches with sizes ranging from 200 nm to 2 µm in width. The masking materials was negative DUV resist: NUV 2300-0.5 of approximately 500 nm. The process flow can be seen here: [[:File:Process_flow_for_test_wafers xx.pdf]] | ||
==Etched close to optimal== | ==Etched close to optimal== | ||
Revision as of 17:02, 18 February 2025
Feedback to this page': click here
THIS PAGE IS UNDER CONSTRUCTION
Made by Berit bghe @ DTU Nanolab
Using the standard Cr etch recipe I was etching through 100 nm Cr on a 150 mm wafer it an etch load of 50%
I recorded the end point signal and tried three different stopping times to figure out when to stop the etch. I want to find out how I can use the end point signal to get the best etch result; Etch through - also in the small patterns without too much over etch.
I was looking at trenches with sizes ranging from 200 nm to 2 µm in width. The masking materials was negative DUV resist: NUV 2300-0.5 of approximately 500 nm. The process flow can be seen here: File:Process_flow_for_test_wafers xx.pdf
Etched close to optimal
| Middel of the wafer | Close to wafer edge |
|---|---|
|
|
Etched too long
| Middel of the wafer | Close to wafer edge |
|---|---|
|
|
Etched too short
| Middel of the wafer | Close to wafer edge |
|---|---|
|
|