Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-4/Nitride Etch: Difference between revisions
Line 5: | Line 5: | ||
[[Category: Etch (Dry) Equipment|DRIE]] | [[Category: Etch (Dry) Equipment|DRIE]] | ||
<br> {{CC1}} | <br> {{CC1}} | ||
==Etching of silicon rich nitride (SRN) with recipes developed for SiO2 etching== | ==Etching of silicon rich nitride (SRN) with recipes developed for SiO2 etching== |
Revision as of 12:18, 22 August 2023
Feedback to this page:
click here
Unless otherwise stated, this page is written by DTU Nanolab internal
Etching of silicon rich nitride (SRN) with recipes developed for SiO2 etching
Parameter | Recipe name: SiO2_res_10 | Recipe name: DOE2/Post_II_21 |
---|---|---|
Coil Power [W] | 2500 | 3840 |
Platen Power [W] | 300 | 300 |
Platen temperature [oC] | 20 | 20 |
H2 flow [sccm] | 25.6 | 0 |
He flow [sccm] | 448.7 | 0 |
C4F8 flow [sccm] | 25.6 | 30 |
Pressure [mTorr] | 8.8 | 0.9 |
Typical results | SiO2_res_10 | DOE2/Post_II_21 |
---|---|---|
Average etch of SRN on 6" wafer | 166 nm/min [+- 17% over a 6" wafer] | 142 nm/min [+- 9% over a 6" wafer] |
Etch rate of Si3N4 | ? | ? |
Etch rate of SiO2 | 250 nm/min [+- 3% over a 6" wafer] | 306 nm/min [on small piece] |
Etch rate in Si | ?nm/min | ? nm/min |
Etch rate of Mir resist | ? nm/min | ? nm/min |