Jump to content

Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-4/Nitride Etch: Difference between revisions

From LabAdviser
Bghe (talk | contribs)
Bghe (talk | contribs)
Line 18: Line 18:
|Coil Power [W]
|Coil Power [W]
|2500
|2500
|200
|3840


|-
|-
|Platen Power [W]
|Platen Power [W]
|300
|300
|50
|300


|-
|-
Line 33: Line 33:
|H2 flow [sccm]
|H2 flow [sccm]
|25.6
|25.6
|15
|0
|-
|-
|He flow [sccm]
|He flow [sccm]
Line 47: Line 47:
|Pressure [mTorr]
|Pressure [mTorr]
|8.8
|8.8
|10
|0.9


|-
|-

Revision as of 12:33, 22 August 2023

Feedback to this page: click here
Template:CC1

THIS PAGE IS UNDER CONSTRUCTION

Etching of silicon rich nitride (SRN) with recipes developed for SiO2 etching

Parameter Recipe name: SiO2_res_10 Recipe name: DOE2/Post_II_21
Coil Power [W] 2500 3840
Platen Power [W] 300 300
Platen temperature [oC] 20 20
H2 flow [sccm] 25.6 0
He flow [sccm] 448.7 0
C4F8 flow [sccm] 25.6 30
Pressure [mTorr] 8.8 0.9
Typical results SiO2_res_10 DOE2/Post_II_21
Etch of SRN ~43nm/min [measured 39-50 nm/min over a 6" wafer] 23-25 nm/min [4" on carrier]]
Etch rate of Si3N4 ~49 nm/min [4" on carrier] 24-26 nm/min [4" on carrier]
Etch rate of SiO2 ~42nm/min [41-43 nm/min over a 6" wafer] 13.7-14.7 nm/min [4" on carrier]
Etch rate in Si ñm/min 11-13 nm/min (10% load, 4" wafer on 6" carrier)
Etch rate of Mir resist ~nm/min ~17 nm/min
Tested etch time without burning the resist 3 min (6 min => resist burned) 30 min
Profile [o]