Line 27: Line 27:
|-
|-
|1PBSG
|1PBSG
|
|17
|
|1600
|
|0
|
|135
|
|40
|
|500
|
|800LF
|Developed for waveguide top cladding by ''Haiyan Ou @DTU Photonics''
|Developed for waveguide top cladding by ''Haiyan Ou @DTU Photonics''
|-
|BGE_PBSG
|17
|1600
|0
|240
|60
|500
|800LF
|Low stress PBSG
|-
|-
|}
|}

Revision as of 08:49, 8 December 2010

At the moment DANCHIP has 3 PECVDs that can deposite silicon oxide with or without dopants of Boron, Phosphorous or Germanium. PECVD1 and PECVD3 are for silicon based processing. PECVD2 is for III-V processing and is described under III-V processing. Look at the PECVD page to learn more about the PECVDs at DANCHIP. All though PECVD1 and PECVD3 are very much alike you cannot count on the a recipe on one system will give exactly the same results on the other system.


Recipes on PECVD1 for deposition of silicon oxides

Recipes

Recipe name SiH4 flow [sccm] N2O flow [sccm] N2 flow [sccm] B2H6 flow [sccm] PH3 flow [sccm] Pressure [mTorr] Power [W] Description
1oxide/1ox_std/standard 17 1600 0 0 0 400 380LF Process control recipe. Developed for waveguides
1PBSG 17 1600 0 135 40 500 800LF Developed for waveguide top cladding by Haiyan Ou @DTU Photonics
BGE_PBSG 17 1600 0 240 60 500 800LF Low stress PBSG

Expected results

Recipe name Deposition rate [µm/min] RI Uniformity [%] Comments
1oxide/1ox_std/standard ~0.193 1.46 2 The latest measured values can be seen in the process control sheet in LabManager
1PBSG ~0.3


Recipes on PECVD3 for deposition of silicon oxides

Recipes

Recipe name SiH4 flow [sccm] N2O flow [sccm] N2 flow [sccm] Pressure [mTorr] Power [W] Description
LFSiO 12 1420 392 550 60

LF=Low Frequency

Expected results

Recipe name Deposition rate [nm/min] RI Uniformity [%]
LFSiO ~81 ~1.48 <1