Chromium can be thermally evaporated in the [[Specific_Process_Knowledge/Thin_film_deposition/thermalevaporator|Thermal Evaporator]] (NANO 36 THERMAL EVAPORATOR SYSTEM). At DTU Nanolab, we use dedicated 4" long chromium plated tungsten rods (supplier: KJLC). During power ramp up, the material warms up and sublimates. Unlike deposition of Al and Ag, where simple crucibles are used with point-source evaporation from bottom to the substrate, the deposition of chromium proceeds in all directions. To prevent the deposition on the side-walls and the bottom of the chamber a specific protecting shield is mounted beneath the tungsten rod.
Chromium can be thermally evaporated in the [[Specific_Process_Knowledge/Thin_film_deposition/thermalevaporator|Thermal Evaporator]] (NANO 36 THERMAL EVAPORATOR SYSTEM). At DTU Nanolab, we use dedicated 4" long chromium plated tungsten rods (supplier: KJLC). During power ramp up, the material warms up and sublimates. Unlike deposition of Al and Ag, where simple crucibles are used with point-source evaporation from bottom to the substrate, the deposition of chromium proceeds in all directions. To prevent the deposition on the side-walls and the bottom of the chamber a specific protecting shield is mounted beneath the tungsten rod.


The shield design was developed by Henrik Nielsen (Nanolab, ThinFilm), and build by Nanolab Facility service. The process was developed and tested by Evgeniy Shkondin (Nanolab, ThinFilm) in december 2020.
 
<b>The shield design was developed by Henrik Nielsen (Nanolab, ThinFilm), and build by Nanolab Facility service. The process was developed and tested by Evgeniy Shkondin (Nanolab, ThinFilm) in december 2020.</b>
 


<gallery caption="" widths="600px" heights="400px" perrow="2">
<gallery caption="" widths="600px" heights="400px" perrow="2">

Revision as of 15:17, 29 May 2021

Thermal evaporation of Chromium

Chromium can be thermally evaporated in the Thermal Evaporator (NANO 36 THERMAL EVAPORATOR SYSTEM). At DTU Nanolab, we use dedicated 4" long chromium plated tungsten rods (supplier: KJLC). During power ramp up, the material warms up and sublimates. Unlike deposition of Al and Ag, where simple crucibles are used with point-source evaporation from bottom to the substrate, the deposition of chromium proceeds in all directions. To prevent the deposition on the side-walls and the bottom of the chamber a specific protecting shield is mounted beneath the tungsten rod.


The shield design was developed by Henrik Nielsen (Nanolab, ThinFilm), and build by Nanolab Facility service. The process was developed and tested by Evgeniy Shkondin (Nanolab, ThinFilm) in december 2020.


Set-up installation

The deposition of Chromium requires a major change of the tool hardware installation. Ask Nanolab responsible employee if you need to perform this change.

Recipe and process performance

Deposition rate (Å/s) 1*
Maximum Thickness 100 nm**
Film Tooling 173 %
Density 7.2 g/cm3
Z-factor 0.305

* The deposition rate can be increased (up to 2Å/s or even 5 Å/s), but it requires a new recipe.

**Although it is possible to deposit 100 nm, we do not recommend exceeding the thickness setpoint above 80 nm, due to instabilities at the end.


Deposition of 100 nm

The adjusted tooling factor 173%. Full 6" wafer is loaded with shadow-mask. Deposition thickness setpoint is set to 100 nm.

Pressure fluctuations during the ramp-up:

  • Rise 1 phase @ 0-15W: 4.4 10-6 Torr → 6.2 10-6 Torr
  • Soak 1 phase @ 15W: 6.2 10-6 Torr → 10-5 Torr → 6.5 10-6 Torr
  • Rise 2 phase @ 15-24W: 6.5 10-6 Torr → 1.3 10-5 Torr → 1.6 10-6 Torr
  • Soak 2 phase @ 24W: 1.6 10-6 Torr → 1.8 10-6 Torr


Pressure (Torr) Deposition rate (Å/s) Output power (W) Deposited thickness (nm) Comment
2.3 10-6 1.0 24.5 0 fine
9.2 10-7 0.97 25 10 fine
8.8 10-7 0.98 25.6 20 fine
9.9 10-7 0.98 26.0 30 fine
1.2 10-6 0.99 26.3 40 fine
1.3 10-6 1.0 26.6 50 fine
1.4 10-6 0.99 26.7 60 fine
1.4 10-6 0.99 26.8 70 fine
1.4 10-6 1.03 26.6 80 fine
1.6 10-6 0.97 25.7 90 Cr retraction starts from the center point of the rod
2.5 10-6 1.02 27.4 100 (10% opened area) Pressure fluctuates a little the last 10 nm.



Figure 8. Thickness distribution across 6" wafer. Measurement is performed using Dektak profilometer.


At the end of the lifetime (deposition in the range of 80-100nm at the given rate and set-up conditions) the Cr starts to detract from the tungsten rod leaving an empty area that illuminates a very bright light. It is not always that the retraction begins from the middle, there are cases where it starts from one of the edges. In such a case, the deposition is a bit unstable in terms of measured power and pressure.

Film characterisation

Full 6" wafer is loaded for film characterization. Measured base pressure before start 4.4 10-6 Torr. Waited 1 hour before start. Deposition thickness setpoint is set to 100 nm.

X-ray reflectivity method

XRR measurements for Cr film has been performed using Rigaku XRD SmartLab diffractometer.


The following model is selected for XRR fitting: Native chromium oxide, bulk chromium layer, native silicon oxide, and the bulk silicon substrate.


Layer name Thickness (nm) Density (g/cm3) Roughness (nm)
CrOx 4.636 4.95362 3.107
Cr

101.6

6.38 2.5
SiO2 1.02 2.19147 0.5
Si 2.33 0.02

In-Plane X-ray diffraction

In-Plane diffraction spectrum acquired with Rigaku XRD SmartLab diffractometer. Incident angle ω=0.4o IS=0.1mm, RS1=RS2=open. Scan speed: 1o/min.

X-ray photoelectron spectroscopy

XPS profiles for Al films has been obtained using XPS K-Alpha equipment.


SEM and AFM

SEM and AFM measurements illustrate surface morphology and roughness.