Specific Process Knowledge/Thin film deposition/Lesker: Difference between revisions
Line 141: | Line 141: | ||
''By Bjarke Thomas Dalslet @Nanotech.dtu.dk'' | ''By Bjarke Thomas Dalslet @Nanotech.dtu.dk'' | ||
The Lesker CMS 18 sputter system provides thin films of varying surface roughness. This roughness was verified to be dependent on the sputtered material, sputter mode (DC or RF) and the substrate bias strength. Other probable factors include sputter power and pressure | The Lesker CMS 18 sputter system provides thin films of varying surface roughness. This roughness was verified to be dependent on the sputtered material, sputter mode (DC or RF) and the substrate bias strength. Other probable factors include sputter power and pressure. | ||
The | The surface roughness dependence on a range of sputter parameters can be found in the following pages for: | ||
*[[Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Silicon_Oxide/Deposition_of_Silicon_Oxide_using_Lesker_sputter_tool|SiO<sub>2</sub>]] | |||
The "Ta" study was done on clean Si substrates. The sputter pressure was 3 mTorr using DC sputtering of a Ta target. Some O<math>_2</math> was added to wafer 25 and 26 to make Ta<math>_2</math>O<math>_5</math>. In order to get fully oxidized films, up to 30-45% O<math>_2</math> should be added. Consult the thesis of Carsten Christensen for details on Ta<math>_2</math>O<math>_5</math>. | The "Ta" study was done on clean Si substrates. The sputter pressure was 3 mTorr using DC sputtering of a Ta target. Some O<math>_2</math> was added to wafer 25 and 26 to make Ta<math>_2</math>O<math>_5</math>. In order to get fully oxidized films, up to 30-45% O<math>_2</math> should be added. Consult the thesis of Carsten Christensen for details on Ta<math>_2</math>O<math>_5</math>. | ||
Line 151: | Line 151: | ||
Other studies on metals (NiFe/MnIr) show only limited effect of the substrate bias on the roughness. | Other studies on metals (NiFe/MnIr) show only limited effect of the substrate bias on the roughness. | ||
Line 202: | Line 179: | ||
|- | |- | ||
|} | |} | ||
==Stress in deposited films== | ==Stress in deposited films== |
Revision as of 11:00, 25 March 2020
Feedback to this page: click here
LESKER Sputter Tool
The purpose of the "Sputter-system (Lesker)" is to deposit magnetic metals and dielectrica on a single 4" or 6" wafer at a time.
It can be a problem to take wafers from the sputter system and into the other machines in the cleanroom since the sputter system is not very clean. In principle sputtering should therefore be the last step before you take your wafers out of the cleanroom. If you need to process your wafers further please contact the Thin Film group so they can help you.
Lift-off of magnetic materials should never be done in the normal lift-off bath in Cleanroom D-3. It should always be done in the dedicated lift-off bath in the fumehood next to the sputter system.
The user manual, user APV and contact information can be found in LabManager:
Sputter-System(Lesker) in LabManager
Materials for sputtering
- Gold (Au)
- Nickel (Ni)
- Silver (Ag)
- Silicon (Si)
- NiV alloy
- Iron (Fe)
- + many more (see list below or ask)
Contact the Thin Film group if you have special needs (thinfilm@danchip.dtu.dk).
Sputter rate
The sputter rate depends on
- target material
- gun power (increasing power gives in general higher rate). Be aware of limitations on the power for different materials.
- chamber pressure (increasing pressure gives in general lower rate). Too low a pressure can make the plasma unstable.
- gas in chamber (Ar, N2, O2 or mixture).
In the table below (Relative Sputter rates) there is a list of relative sputter rates for different materials (Al is set to 1). This means that you can estimate the sputter rate for a new material if you have the rate for another material under the same conditions (may only work for non-reactive sputtering, i.e., with Ar as the gas).
Thickness uniformity
We have measured the thickness of a TiOx film deposited on a 6" Si wafer. The thickness measurement was done in the VASE ellipsometer.
Deposition parameters were:
Recipe | source 3 with oxygen |
---|---|
time | 600 s |
Gas | O2/Ar Ratio 10/100 |
Pressure | 3 mtorr |
Gun | 3 |
Target | Ti |
Power | 200 W |
Voltage | 370V |
Date | November 3rd 2015 |
Purpose | Deposition of magnetic metals and dielectrica |
|
---|---|---|
Performance | Film thickness |
|
Deposition rates |
| |
Process parameter range | Process Temperature |
|
Process pressure |
| |
Process Gases |
| |
Substrates | Batch size |
|
Substrate material allowed |
| |
Material allowed on the substrate |
|
* For temperatures above 400°C, please contact thinfilm@danchip.dtu.dk, as higher temperatures may damage the machine.
Film quality optimization
By Bjarke Thomas Dalslet @Nanotech.dtu.dk
The Lesker CMS 18 sputter system can produce films in a wide range of crystalline qualities. The crystalline quality of a film depends strongly on the substrate (lattice matching), but also on the energy the sputtered material can utilize for annealing.
You will find detailed information on film quality optimization for NiFe films here.
Surface roughness optimization
By Bjarke Thomas Dalslet @Nanotech.dtu.dk
The Lesker CMS 18 sputter system provides thin films of varying surface roughness. This roughness was verified to be dependent on the sputtered material, sputter mode (DC or RF) and the substrate bias strength. Other probable factors include sputter power and pressure.
The surface roughness dependence on a range of sputter parameters can be found in the following pages for:
The "Ta" study was done on clean Si substrates. The sputter pressure was 3 mTorr using DC sputtering of a Ta target. Some OFailed to parse (SVG (MathML can be enabled via browser plugin): Invalid response ("Math extension cannot connect to Restbase.") from server "https://wikimedia.org/api/rest_v1/":): {\displaystyle _2}
was added to wafer 25 and 26 to make TaFailed to parse (SVG (MathML can be enabled via browser plugin): Invalid response ("Math extension cannot connect to Restbase.") from server "https://wikimedia.org/api/rest_v1/":): {\displaystyle _2}
OFailed to parse (SVG (MathML can be enabled via browser plugin): Invalid response ("Math extension cannot connect to Restbase.") from server "https://wikimedia.org/api/rest_v1/":): {\displaystyle _5}
. In order to get fully oxidized films, up to 30-45% OFailed to parse (SVG (MathML can be enabled via browser plugin): Invalid response ("Math extension cannot connect to Restbase.") from server "https://wikimedia.org/api/rest_v1/":): {\displaystyle _2}
should be added. Consult the thesis of Carsten Christensen for details on TaFailed to parse (SVG (MathML can be enabled via browser plugin): Invalid response ("Math extension cannot connect to Restbase.") from server "https://wikimedia.org/api/rest_v1/":): {\displaystyle _2}
OFailed to parse (SVG (MathML can be enabled via browser plugin): Invalid response ("Math extension cannot connect to Restbase.") from server "https://wikimedia.org/api/rest_v1/":): {\displaystyle _5}
.
Other studies on metals (NiFe/MnIr) show only limited effect of the substrate bias on the roughness.
Ta
Wafer nr | RF bias (W) | Reactive O2 (%) | Power(W) | Rq (RMS) (nm) | Thickness |
blank1 | 0 | 0 | 180 | 0.209 | |
16 | 10 | 0 | 180 | 0.36 | 56 |
24 | 20 | 0 | 180 | 0.357 | |
25 | 20 | 9 | 180 | 0.202 | 110 |
26 | 20 | 5 | 180 | 0.194 | 95 |
27 | 15 | 0 | 180 | 0.413 | |
28 | 25 | 0 | 180 | 0.164 | |
31 | 30 | 0 | 180 | 0.3 |
Stress in deposited films
Sputter deposition causes stress in the deposited material. Depending on the sputter parameters, the stress can be either tensile or compressive. In 2017 Radu Malureanu investigated the stress in Si, Cr and Cu films deposited with the Lesker sputter system under a range of circumstances.
Results of the study may be found here:
List of available targets for the Sputter-System(Lesker) (03 June 2013)
Deposition material | target thickness | Purity | Max. Power (W) | Max Ramp up and down (W/s) |
Ag | 0,250" | 99,9% | 314 | 20 |
Al | 0,250" | 99,99% | 314 | 20 |
Au | 0,125" | 99,999% | 314 | 20 |
Co | 0,0625" | 99,95% | 126 | 10 |
Cr | 0,125" | 99,95% | 251 | 20 |
Cu | 0,250" | 99,99% | 314 | 20 |
Fe | 0,0625" | 99,9% | 126 | 10 |
Ge | 0,250" | 99,999% | 126 | 0.5 |
Mg | 0.250" | 99,95% | 215 | 20 |
Mo | 0,250" | 99,95% | 314 | 20 |
Nb | 0,250" | 99,95% | 314 | 20 |
Ni | 0,125" | 99,9% | 188 | 10 |
Pd | 0,125" | 99,95% | 251 | 20 |
Pt | 0,125" | 99,95% | 251 | 20 |
Ru | 0,125" | 99,95% | 314 | 20 |
Si, Undoped | 0,250" | 99,999% | 126 | 0.5 |
Ta | 0,250" | 99,95% | 314 | 20 |
Te | 0,250" | 99,999% | 16 | 0.5 |
Ti | 0,250" | 99,7% | 251 | 20 |
Al2O3 | 0,125" + Cu backing plate | 99,99% | 63 | 0.5 |
Al2O3 | 0,250" | 99,99% | 63 | 0.5 |
Al/Cu99,5/0,5% | 0,250" | 99,99% | 314 | 20 |
Co/Fe 50/50% | 0,0625" | 99,95% | 126 | 10 |
Co/Fe 80/20% | 0,0625" | 99,95% | 126 | 10 |
Co/Fe 90/10% | 0,0625" | 99,95% | 126 | 10 |
Cr2O3 | 0,125" + Cu backing plate | 99,8% | 63 | 0.5 |
Cu/Ti/25% | 0,125" | 99,99% | 251 | 20 |
Fe/Mn 50/50% | 0,250" | 99,95% | 126 | 10 |
ITO (In2O3/SnO2) 90/10% | 0,125" | 99,99% | 63 | 0.5 |
Mn/Ir80/20% | 0,125" | 99,9% | 251 | 20 |
MgO | 0,125" | 99,95% | 63 | 0.5 |
Ni/Co50/50% | 0,0625" | 99,95% | 126 | 20 |
Ni/Co 50/50% | 0,125" | 99,95% | 126 | 20 |
Ni/Fe 80/20% | 0.125" | 99,95% | 126 | 20 |
NiV 93/7% | 0,250" | 99,95% | 157 | 20 |
SiC | 0,125" + Cu backing plate | 99,5% | 63 | 0.5 |
Si3N4/MgO 2% | 0,125" | 99,9% | 63 | 0.5 |
SiO2 | 0,125" | 99,995% | 126 | 0.5 |
SiO2 | 0,250" | 99,995% | 126 | 0.5 |
Ta2O5 | 0,125" | 99,900% | 63 | 0.5 |
AZO (ZnO/Al2O3) 98%/2% | 0,125" | 99,99% | 126 | 0.5 |
ZnO | 0.250" | 99,999% | 63 | 0.5 |
ZrO(2)/Y(2)O(3) | 99,900% | 63 | 0.5 | |
V | 0.125" | 99,500% | 188 | 20 |
W | 0.250" | 99,500% | 314 | 20 |
Hf | 0.125" | - | 188 | 20 |
Sn | 0.250" | - | 31 | 0.5 |
Relative Sputter rates
To use these charts, locate the material for which known conditions are available. Then multiply the rate by the relative factors to arrive at the estimated rate for the new material. For example, with previous data showing 3.5Å/s Aluminum at 100W, then Titanium at similar conditions will generate approximately
- (0.53/1.00)·3.5 Å/s ≅ 2 Å/s
The rates in this table are calculated based on a 500V cathode potential. As the power is increased greater than two times the original rate, then the relative rate will drop slightly (up to 10%). For example, Aluminum at 250W
- Al250W = 0.9·Al100W·(P1/P0)
- 0.9·3.5 Å/s·(250/100) ≅ 7.4 Å/s
The rates in the ceramics table assume the use of an RF power supply and account for the partial duty cycle of the RF generator as compared to a DC supply.
Metals and semiconductors
Deposition material | name | Relative depostion rate |
Ag | Silver | 2.88 |
Al | Aluminum** | 1.00 |
Au | Gold | 1.74 |
Be | Beryllium | 0.21 |
C | Carbon | 0.23 |
Cu | Copper | 1.42 |
GaAs | Gallium Arsenide {100} | 1.03 |
GaAs | Gallium Arsenide {110} | 1.03 |
Ge | Germanium | 1.50 |
Mo | Molybdenum | 0.66 |
Nb | Niobium | 0.76 |
Pd | Palladium | 1.77 |
Pt | Platinum | 1.00 |
Re | Rhenium | 0.84 |
Rh | Rhodium | 1.16 |
Ru | Ruthenium | 0.98 |
Si | Silicon | 0.60 |
Sm | Samarium | 1.74 |
Ta | Tantalum | 0.67 |
Th | Thorium | 1.31 |
Ti | Titanium | 0.53 |
V | Vanadium | 0.50 |
W | Tungsten | 0.57 |
Y | Yttrium | 1.53 |
Zr | Zirconium | 0.88 |
Oxides and Ceramics
Deposition material | name | Relative depostion rate |
Al2O3 | Alumina | 0.05 |
SiC | Silicon Carbide | 0.22 |
SiO2 | Silicon Dioxide | 0.21 |
TaC | Tantalum Carbide | 0.09 |
Ta2O5 | Tantalum Pentoxide | 0.39 |
Magnetic Materials
Deposition material | name | magn. | Relative depostion rate |
Co | Cobalt | Low | 0.73 |
Cr | Chromium | Med | 0.87 |
Fe | Iron | High | 0.57 |
Mn | Manganese | Med | 0.14 |
Ni | Nickel | Low | 0.86 |
Ni80Fe20 | Permalloy | High | 0.80 |