Specific Process Knowledge/Etch/DRIE-Pegasus/picoscope: Difference between revisions
Appearance
| Line 1: | Line 1: | ||
'''Feedback to this page: | |||
[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Etch/DRIE-Pegasus/picoscope click here]''' | |||
[[Category: Equipment |Etch DRIE]] | |||
<--comment --> | |||
= Process optimization using the Picoscope = | = Process optimization using the Picoscope = | ||
| Line 35: | Line 39: | ||
|- | |- | ||
|} | |} | ||
When running any recipe on theSPTS Pro software | |||
Using the SPTS Pro soft | |||
<gallery caption="4 cycles of Process A " widths="400" heights="500" perrow="2"> | <gallery caption="4 cycles of Process A " widths="400" heights="500" perrow="2"> | ||
Revision as of 13:21, 17 March 2020
Feedback to this page: click here <--comment -->
Process optimization using the Picoscope
The original standard recipes on Pegasus 1 differ in many ways. The second step of one of them is listed below:
| Process A Step 2 parameters | ||
|---|---|---|
| Parameter | Etch | Dep |
| Gas flow (sccm) | SF6 350 (1.5 s), 550 | C4F8 200 |
| Cycle time (secs) | 7.0 | 4.0 |
| Pressure (mtorr) | 25 (1.5 s), 150 | 25 |
| Coil power (W) | 2800 | 2000 |
| Platen power (W) | 140 (1.5) 45 | 0 |
| Common | Temperature 20 degs | |
When running any recipe on theSPTS Pro software Using the SPTS Pro soft
- 4 cycles of Process A
-
Left: Recorded with the SPTS software
-
Right: Recorded with the Picoscope
- 4 cycles of Process D4
-
Left: Recorded with the SPTS software
-
Right: Recorded with the Picoscope