Based on the results obtained above, a revised adhesion layer model for Ti/Au and Cr/Au thin-�lm systems is proposed. The model is intended as
Based on the results obtained above, a revised adhesion layer model for Ti/Au and Cr/Au thin-film systems is proposed. The model is intended as an improvement in the description of the layer-layer interaction compared to the model described in Fig. 1, with the aim of helping the thin-film engineering of nanodevices. The adhesion layer model is shown in Fig. 5.15. The growth of both adhesion layers starts with the deposition of the atoms on the substrate (1) and the subsequent formation of an amorphous layer (2). During the deposition,
an improvement in the description of the layer-layer interaction compared
both Ti and Cr get partially oxidized by oxygen and water molecules present on the substrate surface and in the deposition chamber. The adhesion layer acts as a wetting layer for Au, reducing the nucleation energy barrier and increasing the number of nucleation sites compared to the case where Au is directly evaporated onto the SiO2 surface. The enhanced wetting is due to the formation of Ti-Au and Cr-Au chemical bonds. This leads to the formation of a continuous film having i) monodisperse grain size and ii) the energetically most favorable [111] crystal orientation for Au (3). For the Cr/Au system there is an extra step: the inter-diffusion between Cr and Au to form a Cr-Au alloy (4). Such diffusion is limited to a thickness of 2-3 nm for samples prepared at room temperature.
to the model described in Section 5.1, with the aim of helping the thin-�lm
 
engineering of nanodevices.
[[File:17.png|500px|thumb|Fig. 1. Revised adhesion layer model for Ti/Au and Cr/Au multilayer systems. (1) Adhesion layer nucleation; (2) growth of a partially oxidized adhesion
The adhesion layer model is shown in Fig. 5.15. The growth of both
layer; (3) growth of Au grains with [111] crystal orientation on top of the adhesion layer; (4) only for Cr: Cr/Au inter-di�usion and alloy formation during/after Au deposition.]]
adhesion layers starts with the deposition of the atoms on the substrate (1)
and the subsequent formation of an amorphous layer (2). During the deposition,
both Ti and Cr get partially oxidized by oxygen and water molecules
present on the substrate surface and in the deposition chamber. The adhesion
layer acts as a wetting layer for Au, reducing the nucleation energy
barrier and increasing the number of nucleation sites compared to the case
where Au is directly evaporated onto the SiO2 surface. The enhanced wetting
is due to the formation of Ti-Au and Cr-Au chemical bonds. This leads
to the formation of a continuous �lm having i) monodisperse grain size and
ii) the energetically most favorable [111] crystal orientation for Au (3). For
the Cr/Au system there is an extra step: the inter-di�usion between Cr and
Au to form a Cr-Au alloy (4). Such di�usion is limited to a thickness of 2-3
nm for samples prepared at room temperature.


= Recommendations for nanodevice fabrication =
= Recommendations for nanodevice fabrication =

Revision as of 13:16, 14 August 2018

Adhesion layers

The deposition of metal thin-film structures on dielectric or semiconductor substrates is important in a wide range of micro/nanofabrication applications (plasmonics, metamaterials, organic transistors, substrates for graphene growth, field effect devices).

Noble metals such as Au, Ag, and Pt are often used for the fabrication of these structures. Noble metals are preferred for their high thermal and electrical conductivities, strong and unique optical resonances in the visible and near-infrared (NIR) region of the electromagnetic spectrum due to the resonant response of their free electrons to the electric field of light, and chemical inertness. However, their chemical inertness is also a problem during the fabrication process, because the layers adhere poorly to the substrate, leading to different phenomena like delamination, peeling and deterioration of device performance over time.

An empiric approach has been applied to the adhesion enhancement, leading to the application of extremely thin adhesion layers between the substrate and the noble metal films. The most used of these adhesion layers are transition metals like Ti and Cr, but the advantages of using these materials as adhesion layers are poorly understood.

Fig. 1 represents the simplified adhesion layer model usually used in the micro and nanofabrication community for a generic bilayer system. In this model, the adhesion layer and the noble metal over-layer are deposited sequentially by PVD and are considered to be completely uniform and in perfect contact. Ti and Cr are known to be more chemically reactive than noble metals and thereby increase the adhesion as they chemically bind to the substrate. However, the model does not include any layer-layer interaction. Moreover, it is considered to be independent of the thin-film thickness. Due to the continuous miniaturization of structures and devices, the total metal thin-film thicknesses have reached tens of nanometers, with the thickness of the over-layer approaching the one of the adhesion layer. In these conditions it is unclear if the simplified model is still adequate.

Here the characterization work carried out on two main thin-film systems, Cr/Au and Ti/Au stacks, is presented.

Fig. 1: Schematic representation of a substrate, adhesion layer and overlayer system. The substrate is either a dielectric or semiconductor material and the over-layer is a metal.

Adhesion layer effect on Au thin films

Effect on Au film morphology, grain size and texture

From the cross section profile of the 2nm Au sample (Fig. 2a), it is clear that Au, when deposited directly on SiO2, in order to reduce the interface energy, forms a nanoparticle-like layer in contrast to a continuous film. The diameter of the nanoparticles is about 10 nm. The nanoparticle morphology is confirmed by AFM analysis (Fig. 2b). The RMS surface roughness was measured to be 2.4 nm. For comparison, the RMS roughness of the SiO2 substrate was 0.3 nm. When the thin-film nominal thickness is increased to 20 nm (20nm Au sample, Fig. 2c), the Au layer becomes continuous, but a certain degree of surface roughness is still present due to grain coalescence. The AFM image (Fig. 2d) shows an RMS surface roughness of 1.0 nm, which is significantly lower than the 2nm Au sample.

Fig. 2: TEM cross section images and 300x300 nm AFM images of the 2nm Au sample (a-b) and of the 20nm Au sample (c-d).

From the TEM bright field cross section analysis of the 2nm Ti/2nm Au sample, it is observed that 2 nm of Ti forms a continuous layer below the Au layer (Fig. 3a). The Au layer is continuous over the Ti, indicating that Ti is responsible for an interface energy decrease, acting as an adhesive. The AFM analysis of the same sample confirmed the continuous structure, and an RMS surface roughness of 0.8 nm was measured (Fig. 3b). The 2nm Ti/20nm Au sample also shows a smoother film compared to the 20nm Au sample (Fig. 3c), and the AFM analysis shows an RMS surface roughness of 0.5 nm (Fig. 3d), very similar to the one of the Si substrate.

In contrast to the case with the Ti adhesion layer, TEM bright field analysis of the 2nm Cr/2nm Au sample shows a single continuous layer (Fig. 4a). The AFM RMS surface roughness is 1.2 nm (Fig. 4b). Increasing the nominal Au thickness to 20 nm for the 2nm Cr/20nm Au sample, the film still presented a single-layer morphology (Fig. 4c), while the RMS surface roughness decreased to 0.6 nm (Fig. 4d).

To investigate the crystal orientation of the metal thin-films, tramsimission Kikuchi diffraction was used (Fig. 5a) (see Transmission Kikuchi diffraction for more information). The nanostructure of the 20nm Au film has a bimodal grain size distribution (Fig. 5b). While the smaller grains have different crystal orientations, the large grains (blue color) all have [111] orientation.

Microstructural evolution and growth of metal thin-films deposited by physical vapor deposition on amorphous dielectric substrates follows island growth. The first thin-film growth step is the nucleation of small islands once the activation barrier and the critical nuclei size have been overcome. It is followed by a second step of island growth, during which the impinging atoms contribute to increase island size. The third step, usually happening simultaneously with step 2, is island coalescence, where a strong driving force is present for coarsening through surface atom diffusion and grain boundaries (GB) motion. During this process, the island growth is driven by the minimization of surface and interface energy.

Fig. 6a represents two Au islands having different crystal orientations. In particular they have the (111)- and (100)-facets, respectively, parallel to the substrate surface. The growth of these islands is dependent on their orientation (Fig. 6b): for Au, which has a face-centered cubic unit cell, the (100) surface has a higher surface energy than the (111) surface, and to minimize energy, the (100) surface grows faster. Islands having (100) or (110) facets parallel to the substrate grow faster in the vertical direction, while islands with (111) facets parallel to the substrate grow faster laterally. The result is a continuous film, having laterally larger and flatter islands with [111] crystal direction, and laterally smaller but taller islands with [100] and [110] orientations.

The samples with the adhesion layers and 20 nm Au layer were also analyzed. The addition of the adhesion layer had in both cases a profound impact on grain size and orientation of the Au film, as visible in Fig. 7a and 7c. The image shows small grains mainly oriented in the [111] crystal direction, with an average grain size of 40 nm for Ti (Fig. 7b) and 36 nm for Cr (Fig. 7d). During the collection of the TKD maps, only the Kikuchi patterns produced by the electron scattering from the Au layer were recorded and indexed. Cr and Ti layers did not contribute to the pattern formation due to two main reasons: i) they are too thin to produce enough scattered electrons and ii) they are worse electron scattering centers tahn Au because they have a lower atomic number.

Fig. 7: TKD IPFZ maps of the growth direction and grain size distributions of the 2-Ti/20-Au sample (a-b) and of the 2-Cr/20-Au sample (c-d).

The smaller grain size is attributed to an enhanced wetting of the deposited Au promoted by the adhesion layer. The enhanced wetting behaviour increases the number of nucleation sites compared to the pure Au film case, where Au is evaporated directly onto the SiO2 surface. This eventually leads to a much denser nucleation of the Au grains, which at the same time facilitates the inter-diffusion of Au atoms. The enhanced wetting might be due to the formation of Ti-Au and Cr-Au bonds.

The very dominant [111] crystal orientation observed implies a decrease of the energy barrier for the formation of the energetically most favourable Au crystal structure. This is promoted by the denser nucleation and stronger inter-diffusion of Au atoms described above. In contrast to the pure Au case, all the grains have the same diffusion rate of the (111) exposed planes, and therefore the grains grow with a narrow grain size distribution. Since the film has been deposited at room temperature, the system did not have enough energy to overcome the energy barrier for grain coalescence, hence resulting in grains with a small average size. For the Cr case, also small grains with [100] and [110] crystal orientations were detected. This might suggest that for Au on Cr the [111] orientation is energetically less favored with respect to the [100] and [110] orientations compared to the Ti/Au case.

Bilayer chemical composition and elemental distribution

The knowledge of the chemical composition and elemental distribution of the bilayer systems is important to understand the type of interaction between

the layers and their di�erent structure. To obtain such information, the bilayer systems were investigated using STEM-EDX, STEM-EELS and XPS depth pro�ling. For the chemical distribution of the elements in the 2-Ti/2-Au sample, the STEM-EDX measurements at the Ti/Au interface showed the presence of a continuous Ti layer below the Au layer (Fig. 5.9a). This result is in good agreement with the TEM micrograph of Fig. 5.5a.

The analysis of the 2-Cr/2-Au sample showed instead the presence of Cr throughout the whole thickness of the Au layer (Fig. 5.9b). Since Cr and Au were deposited sequentially and not by a co-deposition process, this result suggests a strong inter-di�usion. The 2-Cr/20-Au sample was also investigated, to understand the degree of inter-di�usion for a thicker Au layer (Fig. 5.9c). In this case the inter-di�usion between the elements was incomplete, being present for a thickness of 2-3 nm. This suggests that the di�usion process is limited to such a thickness when Cr and Au are deposited at room temperature.

To verify the chemical composition of the samples, in particular to investigate a possible presence of oxygen in the adhesion layer, STEM-EELS analysis was used. A line scan across the layer interfaces of the 2-Ti/2-Au sample shows the presence of a Ti core loss L3 edge at 460 eV and an L2 edge at 465 eV. A SiO2 O-K edge is visible at 538 eV, while the O-K edge of O bounded to Ti is found at 532 eV (Fig. 5.10a).

The same investigation was performed on the 2-Cr/2-Au sample (Fig. 5.10b). The analysis showed a Cr L3 edge at 585 eV and an L2 edge at 594 eV. The SiO2 O-K edge is visible at 545 eV, while at 540 eV a weak OCr-K edge of O bounded to Cr is visible for a limited thickness below Au. Furthermore, the Cr edge presents a compositional tail along the scan direction, which con�rms di�usion into the Au layer. For the length of the tail there is no presence of OCr-K edge, indicating that Cr inside Au is in metallic form. This is in good agreement with the observed di�usion, which involves only metallic Cr.

The source of oxidation of the adhesion layer could have three origins: i) oxidation due to migration of oxygen from the SiO2 substrate, ii) oxidation during the e-beam deposition process, or iii) oxidation due to substrate contamination with water and oxygen molecules. To investigate the oxidation origin, XPS depth pro�le analysis were performed on 2-Ti/20-Au and 2-Cr/20-Au as-deposited samples. The �rst analysis was performed to clarify if oxygen was originating from source i). To rule out possible oxygen migration from the oxygen-rich SiO2 substrate, the metal thin-�lms were deposited on amorphous Si3N4. For both samples, after Ar ion milling of 20 nm of Au, the Au 4f signal intensity decreased and Cr 2p and Ti 2p signals started to appear together with the O 1s signal (Fig. 5.11a for Ti and 5.11b for Cr, respectively). For the Cr case, due to the lower spatial resolution of XPS with respect to STEM-EDX, it was not possible to verify the thickness of Cr-Au inter-di�usion in this case. The XPS electron escape depth at 1486.7 eV for Au is around 0.15 nm [114], meaning that it is not possible to obtain information about interdi �usion for layers thinner than this value without collecting a signal from the underlying material. Peak �ts for the Ti and Cr signals were performed, and are reported in Fig. 5.12. The Ti 2p peak is a convolution of three components: a TiN doublet at 455.0 and 461.1 eV, a TiO2 doublet at 457.7 and 464.0 eV and a TiOx signal, which forms the descending background tail [115]. The �t gives the following information: 1) Ti has formed Ti-N bonds with the Si3N4 substrate; 2) the adhesion layer was partially oxidized during deposition and not from source i). Metallic Ti could not be detected, but its presence cannot be excluded: metallic Ti is highly reactive with respect to oxygen and nitrogen, and the destructive sputtering process used for the depth pro�ling could have enhanced the mixing between Ti, O and N, catalyzing the reaction of the metallic Ti bound to Au to form an oxide or a nitride.

The Cr 2p peak �t is formed by three components: a metallic Cr doublet at 574.4 and 583.6 eV, a Cr2O3 doublet at 576.3 and 585.6 eV and a CrO3 doublet at 580 and 589.2 eV [115]. The result of the �t indicates a partial oxidation of Cr, as in the Ti case.

The second analysis was performed to understand whether the oxygen was originating from source ii) or iii). A 2-Ti/20-Au/2-Ti/20-Au sandwich structure was deposited and analyzed. Both layers of Ti were partially oxidized: the Ti 2p peak signals (Fig. 5.13a) are present at the same depth together with the O 1s signals (Fig. 5.13b). The O 1s signal in the Ti layer in contact with the Si3N4 substrate has higher intensity than the one of the Ti layer between the Au layers. Hence, the Ti layer in contact with the substrate is more oxidized, which suggests that Ti reacted with water adsorbed on the substrate surface. The conclusion is that the oxygen originated from sources ii) and iii).

Water is present in most thin-�lm deposition systems and it is very di�cult to remove because of its capacity to form hydrogen bonds with many materials. Ti reacts with water and oxygen and forms titanium oxides. Furthermore, the use of the same deposition conditions and of the same type of substrate with respect to Ti and a similar chemical reactivity of Ti and Cr suggest that also the Cr layer gets further oxidized by the water and oxygen molecules present on the substrate surface.

Adhesion layer effect on bilayer thin-film electrical resistivity

The change in nanostructure of the Au thin �lm due to the presence of the adhesion layers observed above, could have an important impact on the �lm macroscopic properties such as electrical resistivity. Electrical resistivity in polycrystalline �lms is dependent on electron scattering at surfaces and grain boundaries, and it was expected that the grain size change measured with TKD to be re ected in the electrical properties. Furthermore, for the case of Cr, a Cr-Au alloy was formed, which also was expected to have an impact on the thin-�lm electrical resistivity. To verify these hypotheses, the sheet resistance (R) of the three samples (20-Au, 2-Ti/20-Au, and 2-Cr/20-Au) investigated with TKD above was measured using micro 4-point probe (�4PP). Fig. 5.14a shows that the Ti/Au sample had a lower sheet resistance than pure Au, which can be attributed to the two layers acting as parallel resistors [124]. Data normalization was performed with respect to the average sheet resistance (R) measured at the 20-Au sample. To exclude tip wear e�ects of the �4PP, the measurements were performed measuring with the same probe alternatively

on the 20-Au and 2-Ti/20-Au sample, respectively. Moreover, to rule out thin-�lm thickness variation e�ects, Au TEM crosssection thickness measurements were performed on 36 points along the 20- Au and the 2-Ti/20-Au samples. They revealed a slightly thicker Au �lm thickness in the Ti/Au sample compared to the pure Au �lm (23.6 ±0.5 nm vs 21.9 ±0.5 nm, respectively). Since electrical resistivity is inversely proportional to �lm thickness, the thicker Au �lm contributes to decrease the sheet resistance in the Ti/Au sample with respect to pure Au.

Fig. 5.14b shows that the Cr/Au system had a higher sheet resistance than pure Au. In this case, the formation of a single layer due to Cr-Au inter-di�usion compromised the multilayer assumption. The sheet resistance increase is in line with the general resistivity increase of Cr-Au alloys, which increases linearly with the Cr concentration [125]. Data acquisition and normalization were done as in the Ti/Au case above, and TEM cross-section thickness measurements of the Au layer were done on 29 points of the Cr/Au sample, giving a mean thickness of 22.7 ±0.4 nm. Compared with the thickness of pure Au, this value is slightly higher. However, the sheet resistance decrease due to this thickness di�erence was not enough to compensate the increase due to the Cr-Au alloy formation. The Ti/Au parallel behavior and Cr/Au inter-di�usion seem to have a larger impact on the electrical properties of the multilayer systems than the nanostructure change observed by TKD. For both samples, the increase of grain boundary scattering due to the higher density of grain boundaries, compared to pure Au, could not be measured with setup used, but cannot be excluded a priori.

Adhesion layer model

Based on the results obtained above, a revised adhesion layer model for Ti/Au and Cr/Au thin-film systems is proposed. The model is intended as an improvement in the description of the layer-layer interaction compared to the model described in Fig. 1, with the aim of helping the thin-film engineering of nanodevices. The adhesion layer model is shown in Fig. 5.15. The growth of both adhesion layers starts with the deposition of the atoms on the substrate (1) and the subsequent formation of an amorphous layer (2). During the deposition, both Ti and Cr get partially oxidized by oxygen and water molecules present on the substrate surface and in the deposition chamber. The adhesion layer acts as a wetting layer for Au, reducing the nucleation energy barrier and increasing the number of nucleation sites compared to the case where Au is directly evaporated onto the SiO2 surface. The enhanced wetting is due to the formation of Ti-Au and Cr-Au chemical bonds. This leads to the formation of a continuous film having i) monodisperse grain size and ii) the energetically most favorable [111] crystal orientation for Au (3). For the Cr/Au system there is an extra step: the inter-diffusion between Cr and Au to form a Cr-Au alloy (4). Such diffusion is limited to a thickness of 2-3 nm for samples prepared at room temperature.

File:17.png
Fig. 1. Revised adhesion layer model for Ti/Au and Cr/Au multilayer systems. (1) Adhesion layer nucleation; (2) growth of a partially oxidized adhesion layer; (3) growth of Au grains with [111] crystal orientation on top of the adhesion layer; (4) only for Cr: Cr/Au inter-di�usion and alloy formation during/after Au deposition.

Recommendations for nanodevice fabrication

Nano-optic devices

Nano-electronic devices

Adhesion layer impact on Au �film stability with temperature

allic bond with gold. 5 nm to 10 nm thick of Cr or Ti is commonly used and it is important to deposit Cr or Ti and then immediately Au. If the vacuum chamber is opened in between, the surface of Cr or Ti will get oxidized and that will give a poor adhesion. If a gold layer needs to be deposited directly on Silicon, then native oxide has to be removed by deep in diluted HF and immediately load the evaporation chamber. And after the deposition, the wafer has to be heated op to get some Au-Si diffusion which improves the adhesion.