== | ==Overview of the performance of PECVD thin films and some process related parameters== | ||
{| border="2" cellspacing="0" cellpadding="10" | {| border="2" cellspacing="0" cellpadding="10" | ||
|- | |- | ||
!style="background:silver; color:black;" align="left"|Purpose | !style="background:silver; color:black;" align="left"|Purpose | ||
|style="background:LightGrey; color:black"|Deposition of dielectrica | |style="background:LightGrey; color:black"|Deposition of dielectrica | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*Silicon oxide | *Silicon oxide | ||
| Line 29: | Line 29: | ||
|- | |- | ||
!style="background:silver; color:black" align="left"|Performance | !style="background:silver; color:black" align="left"|Performance | ||
|style="background:LightGrey; color:black"|Film thickness | |style="background:LightGrey; color:black"|Film thickness | ||
|style="background:WhiteSmoke; color:black"| | |||
*~10nm - 30µm | *~10nm - 30µm | ||
|- | |- | ||
|style="background:silver; color:black" | | |style="background:silver; color:black" | | ||
|style="background:LightGrey; color:black"|Index of refraction | |||
|style="background:WhiteSmoke; color:black"| | |||
*~1.4-2.1 | *~1.4-2.1 | ||
|- | |- | ||
|style="background:silver; color:black"| | |style="background:silver; color:black"| | ||
|style="background:LightGrey; color:black"|Step coverage | |||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*In general: Not so good | *In general: Not so good | ||
*PBSG: Floats at 1000<sup>o</sup>C | *PBSG: Floats at 1000<sup>o</sup>C | ||
|- | |- | ||
|style="background:silver; color:black"| | |style="background:silver; color:black"| | ||
|style="background:LightGrey; color:black"|Film quality | |||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*Not so dense film | *Not so dense film | ||
| Line 50: | Line 55: | ||
*300 <sup>o</sup>C | *300 <sup>o</sup>C | ||
|- | |- | ||
|style="background:silver; color:black"| | |style="background:silver; color:black"| | ||
|style="background:LightGrey; color:black"|Process pressure | |||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*~200-900 mTorr | *~200-900 mTorr | ||
|- | |- | ||
|style="background:silver; color:black"| | |style="background:silver; color:black"| | ||
|style="background:LightGrey; color:black"|Gas flows | |||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*SiH<math>_4</math>:0-60 sccm | *SiH<math>_4</math>:0-60 sccm | ||
| Line 72: | Line 79: | ||
*Deposition on one side of the substrate | *Deposition on one side of the substrate | ||
|- | |- | ||
|style="background:silver; color:black"| | |style="background:silver; color:black"| | ||
| style="background:LightGrey; color:black"|Substrate material allowed | |||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*Silicon wafers | *Silicon wafers | ||
| Line 78: | Line 86: | ||
*Quartz wafers | *Quartz wafers | ||
|- | |- | ||
|style="background:silver; color:black"| | |style="background:silver; color:black"| | ||
| style="background:LightGrey; color:black"|Material allowed on the substrate | |||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*Aluminium | *Aluminium | ||
Revision as of 15:09, 7 May 2008
PECVD Plasma Enhanced Chemical Vapor Deposition


We have three PECVD's here at DANCHIP. They can all be used to deposit Silicon oxides and Silicon nitrides with or without dopants of Boron, Phosphorus and Germanium. PECVD1 and PECVD3 are used for silicon based processing where as PECVD2 is dedicated deposition on III-V materials. PECVD1 is the cleanest system where as PECVD3 is allowed to use with substrates with small abouts of metal on. See the precise rules in the equipment manuals which are uploaded in LabManager.
PECVD is a chemical vapor deposition process that applies a plasma to enhance chemical reaction rates of reactive spices. PECVD processing allows deposition at lower temperatures, which is often critical in the manufacture of semiconductors.
All though PECVD1, 2 and 3 are very similar you should not expect to transfer a recipe between the systems and get the same exact same result.
Recipes on PECVD1 and PECVD3
- Recipes on PECVD1 for deposition of silicon oxides
- Recipes on PECVD1 for deposition of silicon nitride and silicon oxynitride
- Recipes on PECVD3 for deposition of silicon oxides
- Recipes on PECVD3 for deposition of silicon nitride and silicon oxynitride
| Purpose | Deposition of dielectrica |
|
|---|---|---|
| Performance | Film thickness |
|
| Index of refraction |
| |
| Step coverage |
| |
| Film quality |
| |
| Process parameter range | Process Temperature |
|
| Process pressure |
| |
| Gas flows |
| |
| Substrates | Batch size |
|
| Substrate material allowed |
| |
| Material allowed on the substrate |
|