LabAdviser/Technology Research/Fabrication of Hyperbolic Metamaterials using Atomic Layer Deposition/AZO gratings: Difference between revisions

From LabAdviser
Eves (talk | contribs)
Eves (talk | contribs)
Line 7: Line 7:
image:AZO_trench_fab.jpg| Scheme of fabrication flow. High aspect ratio Al<sub>2</sub>O<sub>3</sub> and TiO<sub>2</sub> nanogratings.
image:AZO_trench_fab.jpg| Scheme of fabrication flow. High aspect ratio Al<sub>2</sub>O<sub>3</sub> and TiO<sub>2</sub> nanogratings.
</gallery>
</gallery>
== Process flow ==
Description of steps for fabrication of TiO<sub>2</sub> and AL<sub>2</sub>O<sub>3</sub> nanogratings.
{| border="1" cellspacing="1" cellpadding="3" style="text-align: left; width: 925px; height: 220px;"
|-
|-
!colspan="2" border="none" style="background:#6495ED; color:black;" align="center" width="225px"|Step
!width="250px" style="background:#6495ED; color:black"|Description
!width="200px" style="background:#6495ED; color:black"|LabAdviser link
!width="260px" style="background:#6495ED; color:black"|Image showing the step
|-
|-
!1.1
|Plasma surface treatment
|To ensure clean surface, the 100 mm Si wafer is treated by O<sub>2</sub>/N<sub>2</sub> plasma. (Optional step)
|[[Specific_Process_Knowledge/Lithography/Strip#Plasma_Asher_2| Plasma Asher 2]]
|[[image:00_zero (1)_nanogratings.JPG|250x350px|center|]]
|-
|-
|- style="background:#BCD4E6; color:black"
!1.2
|DUV Resist patterning
|DUV
|[[Specific_Process_Knowledge/Lithography/DUVStepperLithography|DUV Stepper Lithography]].
|[[image:00_zero (2)_nanogratings.JPG|250x350px|center|]]
|-
|-
!1.3
|Deep reactive ion etching (DRIE)
|DRIE; [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/DUVetch|Recipe: PolySOI10]]
| [[Specific_Process_Knowledge/Etch/DRIE-Pegasus|DRIE Pegasus]].
|[[image:00_zero (3)_nanogratings.JPG|250x350px|center|]]
|-
|-
|- style="background:#BCD4E6; color:black"
!1.4
|Plasma surface treatment
|To ensure that remainings of DUV resist are gone, samples are treated by O<sub>2</sub>/N<sub>2</sub> plasma. (Optional step)
|[[Specific_Process_Knowledge/Lithography/Strip#Plasma_Asher_2| Plasma Asher 2]].
|
|-
|-
!1.5
|Scanning Electron Microscopy inspection
|By cleaving the sample it is possible to inspect DRIE etched Si trenches in cross-sectional mode
|
[[Specific_Process_Knowledge/Characterization/SEM_Supra_1|SEM Supra 1]]
<br clear="all" />
[[Specific_Process_Knowledge/Characterization/SEM_Supra_2|SEM Supra 2]]
<br clear="all" />
[[Specific_Process_Knowledge/Characterization/SEM_Supra_3|SEM Supra 3]]
|[[image:Si_trenches_nanogratings.jpg|250x350px|center]]
|-
|-
|- style="background:#BCD4E6; color:black"
!1.6
|Atomic Layer Deposition of either Al<sub>2</sub>O<sub>3</sub> or TiO<sub>2</sub>
|Deposition carried at 150C.Thickness is 90 nm.
||Equipment used: [[Specific_Process_Knowledge/Thin_film_deposition/ALD_Picosun_R200|ALD Picosun R200]]. Standard recipes used: [[Specific_Process_Knowledge/Thin_film_deposition/ALD_Picosun_R200/Al2O3_deposition_using_ALD#Al2O3_recipe_for_deposition_on_high_aspect_ratio_structures| Al2O3T]] and [[Specific_Process_Knowledge/Thin_film_deposition/ALD_Picosun_R200/TiO2_deposition_using_ALD#TiO2_deposition_on_trenches| TiO2T]] .
|[[image:00_zero (4)_nanogratings.JPG|250x350px|center]]
|-
|-
!1.7
|Scanning Electron Microscopy inspection
|By cleaving the sample it is possible to inspect ALD coatings deposited on Si trenches in cross-sectional mode
|
[[Specific_Process_Knowledge/Characterization/SEM_Supra_1|SEM Supra 1]]
<br clear="all" />
[[Specific_Process_Knowledge/Characterization/SEM_Supra_2|SEM Supra 2]]
<br clear="all" />
[[Specific_Process_Knowledge/Characterization/SEM_Supra_3|SEM Supra 3]]
|[[image:TiO2_coating_nanogratings.jpg|250x350px|center]]
|-
|-
|- style="background:#BCD4E6; color:black"
!1.8
|Opening of deposited Al<sub>2</sub>O<sub>3</sub> or TiO<sub>2</sub> top layers.
|Etching happens using ICP Metal etcher with Cl<sub>2</sub>/BCl<sub>3</sub> process gasses.
||Equipment used: [[Specific_Process_Knowledge/Etch/ICP_Metal_Etcher|Metal ICP Etcher]].
|[[image:00_zero (6)_nanogratings.JPG|250x350px|center]]
|-
|-
!1.9
|Scanning Electron Microscopy inspection
|By cleaving the sample it is possible to inspect ICP etcher results Si trenches in cross-sectional mode
|
[[Specific_Process_Knowledge/Characterization/SEM_Supra_1|SEM Supra 1]]
<br clear="all" />
[[Specific_Process_Knowledge/Characterization/SEM_Supra_2|SEM Supra 2]]
<br clear="all" />
[[Specific_Process_Knowledge/Characterization/SEM_Supra_3|SEM Supra 3]]
|[[image:TiO2_top_removal_nanogratings.jpg|250x350px|center]]
|-
|-
|- style="background:#BCD4E6; color:black"
!1.10
|Selective etch of Si between ALD  Al<sub>2</sub>O<sub>3</sub> or TiO<sub>2</sub> coatings.
|Si etching proceeds using ICP Metal etcher with isotropic  process based on SF<sub>f</sub> process gas.
||Equipment used: [[Specific_Process_Knowledge/Etch/ICP_Metal_Etcher|Metal ICP Etcher]].
|[[image:00_zero (7)_nanogratings.JPG|250x350px|center]]
|-
|-
!1.11
|Scanning Electron Microscopy inspection of fabricated structure.
|Proof of final result.
|
[[Specific_Process_Knowledge/Characterization/SEM_Supra_1|SEM Supra 1]]
<br clear="all" />
[[Specific_Process_Knowledge/Characterization/SEM_Supra_2|SEM Supra 2]]
<br clear="all" />
[[Specific_Process_Knowledge/Characterization/SEM_Supra_3|SEM Supra 3]]
|[[image:TiO2_grating_nanogratings.jpg|250x350px|center]]
|-
|-
|- style="background:#BCD4E6; color:black"
!1.12
|Ion beam etching. (Optional)
|Additional shape of the top part. 20 mijn etch using recipe [[Specific_Process_Knowledge/Etch/IBE⁄IBSD_Ionfab_300/IBE_Ti_etch|"Ti acceptance"]] there the stage shoud be placed to 0<sup>o</sup> degree. SEM cross section is used for inspection
|[[Specific_Process_Knowledge/Etch/IBE⁄IBSD_Ionfab_300|IBE/IBSD Ionfab 300]]
|[[image:image1004_nanogratings.jpg|250x350px|center]]
|-
|-
|}
<br clear="all" />

Revision as of 12:50, 15 March 2017

Procces flow description

All samples were prepared and characterized in a class 100 cleanroom. Si (100) wafers of 150 mm were used as a substrate. The main steps in the gratings manufacturing are shown in a figure below. First, the silicon trenches were realized by deep reactive ion etching (DRIE). Then, the trenches were ALD coated. After the selective removal of the top parts, the silicon core between ALD coatings was etched away during the last step. The final structure represents the highly anisotropic vertical grating. Each fabrication step was carefully evaluated using cross-sectional scanning electron microscopy (SEM) imaging.


Process flow

Description of steps for fabrication of TiO2 and AL2O3 nanogratings.

Step Description LabAdviser link Image showing the step
1.1 Plasma surface treatment To ensure clean surface, the 100 mm Si wafer is treated by O2/N2 plasma. (Optional step) Plasma Asher 2
1.2 DUV Resist patterning DUV DUV Stepper Lithography.
1.3 Deep reactive ion etching (DRIE) DRIE; Recipe: PolySOI10 DRIE Pegasus.
1.4 Plasma surface treatment To ensure that remainings of DUV resist are gone, samples are treated by O2/N2 plasma. (Optional step) Plasma Asher 2.
1.5 Scanning Electron Microscopy inspection By cleaving the sample it is possible to inspect DRIE etched Si trenches in cross-sectional mode

SEM Supra 1
SEM Supra 2
SEM Supra 3

1.6 Atomic Layer Deposition of either Al2O3 or TiO2 Deposition carried at 150C.Thickness is 90 nm. Equipment used: ALD Picosun R200. Standard recipes used: Al2O3T and TiO2T .
1.7 Scanning Electron Microscopy inspection By cleaving the sample it is possible to inspect ALD coatings deposited on Si trenches in cross-sectional mode

SEM Supra 1
SEM Supra 2
SEM Supra 3

1.8 Opening of deposited Al2O3 or TiO2 top layers. Etching happens using ICP Metal etcher with Cl2/BCl3 process gasses. Equipment used: Metal ICP Etcher.
1.9 Scanning Electron Microscopy inspection By cleaving the sample it is possible to inspect ICP etcher results Si trenches in cross-sectional mode

SEM Supra 1
SEM Supra 2
SEM Supra 3

1.10 Selective etch of Si between ALD Al2O3 or TiO2 coatings. Si etching proceeds using ICP Metal etcher with isotropic process based on SFf process gas. Equipment used: Metal ICP Etcher.
1.11 Scanning Electron Microscopy inspection of fabricated structure. Proof of final result.

SEM Supra 1
SEM Supra 2
SEM Supra 3

1.12 Ion beam etching. (Optional) Additional shape of the top part. 20 mijn etch using recipe "Ti acceptance" there the stage shoud be placed to 0o degree. SEM cross section is used for inspection IBE/IBSD Ionfab 300