Jump to content

Specific Process Knowledge/Etch/KOH Etch: Difference between revisions

From LabAdviser
Mbec (talk | contribs)
Mbec (talk | contribs)
Line 100: Line 100:


!colspan="2" border="none" style="background:silver; color:black;" align="center"|Equipment  
!colspan="2" border="none" style="background:silver; color:black;" align="center"|Equipment  
|style="background:WhiteSmoke; color:black"|<b>KOH3</b>
|style="background:WhiteSmoke; color:black"|<b>KOH2</b>
|style="background:WhiteSmoke; color:black"|<b>KOH2</b>
|style="background:WhiteSmoke; color:black"|<b>KOH1</b>
|style="background:WhiteSmoke; color:black"|<b>KOH1</b>
Line 106: Line 105:
|-
|-
!style="background:silver; color:black;" align="center" width="60" rowspan="2"|Purpose  
!style="background:silver; color:black;" align="center" width="60" rowspan="2"|Purpose  
|style="background:LightGrey; color:black"|Wet etch of Silicon
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Etch of Silicon in 28 wt% KOH
*Etch of Silicon in 28 wt% KOH
Line 118: Line 116:
|-
|-
|style="background:LightGrey; color:black"|Link to safety APV and KBA
|style="background:LightGrey; color:black"|Link to safety APV and KBA
|style="background:WhiteSmoke; color:black"|
*:[http://labmanager.danchip.dtu.dk/d4Show.php?id=1906&mach=248 see APV here]
*:[http://kemibrug.dk/KBA/CAS/106882/?show_KBA=1&portaldesign=1 see KBA here]
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*:[http://labmanager.danchip.dtu.dk/d4Show.php?id=1906&mach=49 see APV here]
*:[http://labmanager.danchip.dtu.dk/d4Show.php?id=1906&mach=49 see APV here]
Line 133: Line 128:
!style="background:silver; color:black" align="center" valign="center" rowspan="5"|Performance
!style="background:silver; color:black" align="center" valign="center" rowspan="5"|Performance
|style="background:LightGrey; color:black"|Etch rates in crystalline silicon (100)
|style="background:LightGrey; color:black"|Etch rates in crystalline silicon (100)
|style="background:WhiteSmoke; color:black"|
*0.4 µm/min (60 °C)
*0.7 µm/min (70 °C)
*1.3 µm/min (80 °C)
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*0.4 µm/min (60 °C)
*0.4 µm/min (60 °C)
Line 149: Line 140:
|-
|-
|style="background:LightGrey; color:black"|Etch rates in Thermal SiO2  
|style="background:LightGrey; color:black"|Etch rates in Thermal SiO2  
|style="background:WhiteSmoke; color:black"|
*Theoretical values:
*1.2 nm/min (60 °C)
*6 nm/min (80 °C)
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Theoretical values:
*Theoretical values:
Line 161: Line 148:
|-
|-
|style="background:LightGrey; color:black"|Etch rates in SiN  
|style="background:LightGrey; color:black"|Etch rates in SiN  
|style="background:WhiteSmoke; color:black"|
*0.02 nm/min (80 °C)<sup>{{fn|1}}</sup>
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
Line 168: Line 153:
|-
|-
|style="background:LightGrey; color:black"|Roughness
|style="background:LightGrey; color:black"|Roughness
|style="background:WhiteSmoke; color:black"|
*Typical: 100-600 Å
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Typical: 100-600 Å
*Typical: 100-600 Å
Line 178: Line 161:
|-
|-
|style="background:LightGrey; color:black"|Anisotropy
|style="background:LightGrey; color:black"|Anisotropy
|style="background:WhiteSmoke; color:black"|
*The etch rate is very dependent on the crystal orientation of the silicon.
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*The etch rate is very dependent on the crystal orientation of the silicon.
*The etch rate is very dependent on the crystal orientation of the silicon.
Line 189: Line 170:
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Process parameter range
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Process parameter range
|style="background:LightGrey; color:black"|Chemical solution
|style="background:LightGrey; color:black"|Chemical solution
|style="background:WhiteSmoke; color:black"|
*Mixing ratios giving 28 wt% KOH solutions
KOH:H<sub>2</sub>O - 500 g : 1000 ml, when using pills
KOH:H<sub>2</sub>O - 1000 ml: 1200 ml, when using premixed 50% KOH solution
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Mixing ratios giving 28 wt% KOH solutions
*Mixing ratios giving 28 wt% KOH solutions
Line 205: Line 182:
|-
|-
|style="background:LightGrey; color:black"|Temperature
|style="background:LightGrey; color:black"|Temperature
|style="background:WhiteSmoke; color:black"|
*Max 80 °C (standard etch)
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Max 80 °C (standard etch)
*Max 80 °C (standard etch)
Line 216: Line 191:
!style="background:silver; color:black" align="center" valign="center" rowspan="4"|Substrates
!style="background:silver; color:black" align="center" valign="center" rowspan="4"|Substrates
|style="background:LightGrey; color:black"|Batch size
|style="background:LightGrey; color:black"|Batch size
|style="background:WhiteSmoke; color:black"|
*1-25 wafers at a time
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*1-25 wafers at a time  
*1-25 wafers at a time  
Line 226: Line 199:
|-
|-
|style="background:LightGrey; color:black"|Size of substrate
|style="background:LightGrey; color:black"|Size of substrate
|style="background:WhiteSmoke; color:black"|
*4” wafers
*6” wafers
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*4” wafers
*4” wafers
Line 239: Line 209:
|-
|-
|style="background:LightGrey; color:black"|Allowed materials
|style="background:LightGrey; color:black"|Allowed materials
|style="background:WhiteSmoke; color:black"|
*Silicon
*Silicon oxide
*Silicon (oxy)nitride
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Silicon
*Silicon
Line 260: Line 226:
|-
|-
|style="background:LightGrey; color:black"|Masking material
|style="background:LightGrey; color:black"|Masking material
|style="background:WhiteSmoke; color:black"|
*Stoichiometric Si3N4
*Silicon rich nitride SiN
*PECVD Si3N4
*Thermal SiO2
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Stoichiometric Si3N4  
*Stoichiometric Si3N4  

Revision as of 15:05, 23 February 2017

Feedback to this page: click here

THIS PAGE IS UNDER CONSTRUCTION

KOH etch - Anisotropic silicon etch

KOH belongs to the family of anisotropic Si-etchants based on aqueous alkaline solutions. The anisotropy stems from the different etch rates in different crystal directions. The {111}-planes are almost inert whereas the etch rates of e.g. {100}- and {110}-planes are several orders of magnitude faster.

KOH-etching is a highly versatile and cheap way to realize micro mechanical structures if you can live with the necessary Si3N4- or SiO2-masking materials and the potassium contamination of the surface. The latter necessitates in most cases a wet post-clean ('7-up' or RCA-clean) if the wafer is to be processed further.

At Danchip we use as a standard a 28 wt% KOH. The etch rate - and the selectivity towards a SiO2-mask - is depending on the temperature. We normally use T=80 oC but may choose to reduce this to e.g. 60 oC or 70 oC in case of a high-precision timed etch (e.g. defining a thin membrane). In some cases we recommend to saturate the standard 28 wt% KOH with IPA with an etch temperature at T=70 oC (reduce evaporation of IPA). One example is for boron etch-stop, where the selectivity towards the boron-doped silicon is improved compared to the standard etch. Etching with IPA added to the KOH solution can be done in KOH fumehood.


The user manuals, quality control procedures and results, user APVs, technical information and contact information can be found in LabManager:


Si Etch 1: KOH info page in LabManager,

Si Etch 2: KOH info page in LabManager,

Si Etch 3: KOH info page in LabManager

Process Information

Results on V-grooves

Quality Control (QC) for the KOH etching baths.

Quality Control (QC) for KOH1, KOH2 and KOH3
QC Recipe:  
Solution 28 wt% KOH
Temperature 80°C
Time 90 min
Substrate Si (100)
Masking No masking
QC limits KOH1 KOH 2&3
Etch rate in Si(100) 1.3 ± 0.1 µm/min 1.29 ± 0.06 µm/min
Roughness not measured not measured
Nonuniformity < 3% < 3%


KOH etching baths

Key facts for the different etch baths available at Danchip are resumed in the table:


Equipment KOH2 KOH1 KOH Fumehood
Purpose
  • Etch of Silicon in 28 wt% KOH
  • Etch of Silicon in 28 wt% KOH
  • Etch of Silicon in 28 wt% KOH

The bath is dedicated wafer with electroplated Nickel or otherwise dirty wafers

  • Etch of Silicon in user mixed KOH
Link to safety APV and KBA
Performance Etch rates in crystalline silicon (100)
  • 0.4 µm/min (60 °C)
  • 0.7 µm/min (70 °C)
  • 1.3 µm/min (80 °C)
  • 0.4 µm/min (60 °C)
  • 1.3 µm/min (80 °C)

Etch rates might vary due to contamination and poor controlled concentration of the KOH solution

  • Somewhat lower than in the dedicated baths. Approximately 1 µm/min @ 80 °C in 28 wt%
Etch rates in Thermal SiO2
  • Theoretical values:
  • 1.2 nm/min (60 °C)
  • 6 nm/min (80 °C)
Etch rates in SiN
Roughness
  • Typical: 100-600 Å
  • May be high due to contamination and poor controlled concentration of the KOH solution
  • Typical worse than KOH2 and KOH3
Anisotropy
  • The etch rate is very dependent on the crystal orientation of the silicon.
  • The etch rate is very dependent on the crystal orientation of the silicon.
  • The etch rate is very dependent on the crystal orientation of the silicon.
Process parameter range Chemical solution
  • Mixing ratios giving 28 wt% KOH solutions

KOH:H2O - 500 g : 1000 ml, when using pills KOH:H2O - 1000 ml: 1200 ml, when using premixed 50% KOH solution

  • Mixing ratios giving 28 wt% KOH solutions

KOH:H2O - 500 g : 1000 ml, when using pills KOH:H2O - 1000 ml: 1200 ml, when using premixed 50% KOH solution

  • Custom made
Temperature
  • Max 80 °C (standard etch)
  • Max 80 °C
  • Max 80 °C
Substrates Batch size
  • 1-25 wafers at a time
  • 1-25 wafers at a time
  • 1-7 wafers at a time
Size of substrate
  • 4” wafers
  • 4” wafers
  • 2” wafers
  • 4” wafers
  • Small pieces
Allowed materials
  • Silicon
  • Silicon oxide
  • Silicon (oxy)nitride
  • Silicon
  • Silicon oxide
  • Silicon (oxy)nitride
  • Nickel
  • Nickel vanadium alloys
  • Titanium
  • Chromium
  • Gold
  • All except for Polymers
Masking material
  • Stoichiometric Si3N4
  • Silicon rich nitride SiN
  • PECVD Si3N4
  • Thermal SiO2
  • Stoichiometric Si3N4
  • Silicon rich nitride SiN
  • PECVD Si3N4
  • Thermal SiO2
  • Stoichiometric Si3N4
  • Silicon rich nitride SiN
  • PECVD Si3N4
  • Thermal SiO2

1 Measured by Eric Jensen from DTU-Nanotech, October 2013.

Definition of structures

Due to the almost inert (111)-planes it is possible by KOH etching to realize high aspect ratio structures in sigle crytalline silicon using the (111)-planes as sidewalls. In Si(100) these sidewalls are inclined - 54.7o with respect to the (100) surface - whereas in Si(110) the sidewalls are vertical (see figures below).


For Si(100), the relation between the width of the bottom of the etched groove (Wb) and the width of the opening (Wo) at the wafer surface in a groove etched to the depth l is given by:


Wb=Wo2lcot(54.7o)=Wo2l



Definition of <110> alignment structures

The etch rate dependence on the crystallographic planes can be used to determine the <110> crystal directions with high precision (better than +/- 0.05 o). A fast method for doing this, using the symmetric under-etching behavior around but not at the <110>-directions, was described by Vangbo and Bäcklund in J. Micromech. Microeng.6 (1996), 279-284. High-precision control of the <110>-direction during alignment can be necessary in order to control the dimensions of KOH-etched structures (e.g. precise control of V-groove dimensions). A dedicated mask (MASK NAME) has been designed for this purpose.


Etch rates: Empirical formula (Seidl et al)

The following empirical formula can be used for concentrations in the range of 10-60 wt%:

R = k0 [H2O]4 [KOH]0.25 e-Ea/kT,

where k0 = 2480 µm/hr (mol/l)-4.25, Ea = 0.595 eV for Si(100)

and k0 = 4500 µm/hr (mol/l)-4.25, Ea = 0.60 eV for Si(110)