* Long curing at 210°C: BCB210AL.PDF/[[file:BCB210BL.PDF|BCB210BL.PDF]]
* Long curing at 210°C: BCB210AL.PDF/[[file:BCB210BL.PDF|BCB210BL.PDF]]
* Long curing at 250°C: BCB250AL.PDF/[[file:BCB250BL.PDF|BCB250BL.PDF]]
* Long curing at 250°C: BCB250AL.PDF/[[file:BCB250BL.PDF|BCB250BL.PDF]]
Content of BCB250BL.PDF:
<pre>
;
; stored 31.08.2011  at 17:55:33
{P0}
00,00:30,0020,- - - - 3 - - - -,075,250,001,005,028
01,00:10,0020,- - - 2 - - - - -
02,00:30,0020,- - - - 3 - - - -
03,00:10,0020,- - - 2 - - - - -
04,05:00,0050,H - - 2 - - - - -
05,05:00,0050,H C - 2 - - - - -
06,15:00,0100,H - 1 - - - - - -
07,45:00,0100,H C 1 - - - - - -
08,15:00,0150,H - 1 - - - - - -
09,81:00,0150,H C 1 - - - - - -
10,60:00,0250,H - 1 - - - - - -
11,60:00,0250,H C 1 - - - - - -
12,15:00,0020,- C 1 - - - - - -
13,30:00,0020,- C 1 - - - - - -
14,00:00,0010,- C - - - - - - -
</pre>


The AL/BL processes are (should be) identical except for a (2x) pump/purge cycle in the beginning of the BL processes.
The AL/BL processes are (should be) identical except for a (2x) pump/purge cycle in the beginning of the BL processes.