Specific Process Knowledge/Lithography/UVExposure: Difference between revisions
No edit summary |
|||
| Line 189: | Line 189: | ||
[[Image:KSaligner.jpg|300x300px|thumb|The KSaligner MA6 is placed in C-1]] | [[Image:KSaligner.jpg|300x300px|thumb|The KSaligner MA6 is placed in C-1]] | ||
'''Feedback to this section''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/UVExposure# | '''Feedback to this section''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/UVExposure#Aligner:_MA6_-_2 click here]''' | ||
SUSS Mask Aligner MA6 is designed for high resolution photolithography. | SUSS Mask Aligner MA6 is designed for high resolution photolithography. | ||
| Line 195: | Line 195: | ||
Two alignment options are available: top side alignment (TSA) with a split field or a video microscope and back side alignment (BSA) with BSA microscope. It is also possible to make IR- light alignment. | Two alignment options are available: top side alignment (TSA) with a split field or a video microscope and back side alignment (BSA) with BSA microscope. It is also possible to make IR- light alignment. | ||
'''The user manual | '''The user manual, APV, and contact information can be found in [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=339 LabManager].''' | ||
===Process information=== | ===Process information=== | ||
Revision as of 14:14, 6 November 2014
Feedback to this page: click here
UV Exposure Comparison Table
| Equipment | KS Aligner | Aligner-6inch | III-V Aligner | Inclined UV Lamp | |
|---|---|---|---|---|---|
| Purpose |
|
|
|
| |
| Performance | Minimum feature size |
|
|
|
|
| Exposure light/filters/spectrum |
|
|
|
| |
| Exposure mode |
|
|
|
| |
| Substrates | Batch size |
|
|
|
|
| Allowed materials |
|
|
|
| |
Mask for UV exposure
When you do UV exposure you need to have a mask. Here you can find information how to design and order your mask.
Tips and tricks for mask designing
Find a guide for L-edit and mask design here:
Unfortunately they are quite old, but may be useful anyway. Note some links/e-mails etc. are not correct anymore
Alignment marks
Following alignment marks are suggested to use on the EVG620 automatic aligner for good pattern recognition. Pleased be adviced that they can be removed in KOH etching.
- Alignment marks 2 .cif - You need the program "Clewin" to open this file
- Alignment marks 2 .tdb - You need the program "L-Edit" to open this file
External links
Alignment marks location
- KS Aligner MA6
- Aligner 6inch EVG620
The mask's alignment marks for 4inch process:
BSA must be located between -1,0 and +1,0 mm in vertical location from mask center (y=0-+1mm) and exactly at 45mm in left and right in horizontal location (x=+-45mm).
TSA must be located 35-45 mm in left and right in horizontal location and between -2 and +2 mm in vertical location.
The mask's alignment marks for 6inch process:
Both BSA and TSA must be located between -2,5 and +2,5 mm in vertical location from mask center and 60 mm in left and right in horizontal location.
Please notice that if you plan to use the automatic alignment option the alignment marks must be displaced from y=0 to y=+/- 1,6mm.
How to order a mask
Our standard mask supplier is Delta Mask. The smallest feature size obtainable from Delta Mask is 1.5 µm. If you need structures smaller than this please write it specificly in the e-mail. Be aware that this will increase the price by at least a factor of 3.
Send your *.cif file or *.gds file (for 7" mask or masks with CD under 1.5µm only *.gds should be used) in an e-mail along with a text file describing your specs (example spec file). E-mail address can be found in Danchip_contact_information. Cost according to Danchip price list.
Mask sets made by Danchip
Danchip quality control masks
This section contains a description of some of the quality control designs.
ASE standisation designs: The quality control procedure on the ASE is using the daqmask 2 mask
RIE standisation design:
The quality control procedures on RIE2 is using the dASEfeRIE mask
Masks for process development
KS Aligner

Feedback to this section: click here
SUSS Mask Aligner MA6 is designed for high resolution photolithography. The 365nm exposure wavelength version is capable of 1.25 (1.0) um resolution in vacuum contact. All contact exposure programs (vacuum, hard, soft, proximity) are supplied. Two alignment options are available: top side alignment (TSA) with a split field or a video microscope and back side alignment (BSA) with BSA microscope. It is also possible to make IR- light alignment.
The user manual(s), quality control procedure(s) and results and contact information can be found in LabManager.
Process information
The KS Aligner has an i-line notch filter installed. This results in an exposure light peak around 365nm with a FWHM of 7nm. Dependent on the spectral sensitivity of the resist, the optimal dose may be increased compared to broadband exposure on the Aligner-6inch.
Aligner: MA6 - 2
This section is under construction

Feedback to this section: click here
SUSS Mask Aligner MA6 is designed for high resolution photolithography. The 365nm exposure wavelength version is capable of 1.25 (1.0) um resolution in vacuum contact. All contact exposure programs (vacuum, hard, soft, proximity) are supplied. Two alignment options are available: top side alignment (TSA) with a split field or a video microscope and back side alignment (BSA) with BSA microscope. It is also possible to make IR- light alignment.
The user manual, APV, and contact information can be found in LabManager.
Process information
The KS Aligner has an i-line notch filter installed. This results in an exposure light peak around 365nm with a FWHM of 7nm. Dependent on the spectral sensitivity of the resist, the optimal dose may be increased compared to broadband exposure on the Aligner-6inch.
Aligner-6inch
Feedback to this section: click here

Aligner-6inch, EVG620 aligner, is designed for high resolution photolithography. The machine can be used for 2, 4 and 6 inch substrates. Cassette-to-cassette handling option is available only for 6inch substrates. The automatic pattern recognition software is available for the special alignment marks design recommended of EVGroup. Please contact Danchip staff for further information. Available exposure mode: proximity, soft, hard and vacuum contact. Two alignment options are available: top side alignment (TSA) and back side alignment (BSA). IR-light alignment also an option.
The user manual(s), quality control procedure(s) and results and contact information can be found in LabManager
Process information
The Aligner-6inch has a long pass filter designed for SU-8 exposure installed. The SU-8 filter has no transmission in the 250-330nm range, and close to full transmission in the 400-500nm range. In the 350-370nm range, the transmission is approximately 0.5. This results in a broadband exposure light consisting of the i-line (365nm), the h-line (405nm), and the g-line (435nm) from the Hg spectrum. Dependent on the spectral sensitivity of the resist, the optimal dose may be decreased compared to i-line exposure on the KS-Aligner.
III-V Aligner
Feedback to this section: click here
The SÜSS MicroTec MA1006 mask aligner located in the III-V cleanroom is dedicated for processing of III-V compound semiconductors.
Specific use of the mask aligner can be found in the standard resist recipes.

The user manual and contact information can be found in LabManager: Equipment info in LabManager
| Purpose |
Alignment and UV exposure | ||
|---|---|---|---|
| Performance | Exposure mode |
soft contact, hard contact, proximity, flood exposure | |
| Exposure light/filters |
365 nm, 405 nm | ||
| Minimum structure size |
down to 2µm | ||
| Mask size |
| ||
| Alignment modes |
Top side only | ||
| Substrates | Substrate size |
| |
| Allowed materials |
III-V materials | ||
| Batch |
1 | ||
Inclined UV Lamp
Feedback to this section: click here

The Inclined UV lamp is 1000 W Hg(Xe)lamp source designed for near UV, 350-450nm, mid UV, 260-320nm, and deep UV, 220-260nm exposures of resists and polymers. The exposure source can be also used to make an inclined exposure in air or in the media tank.
The tool was purchased in February 2009 from Newport. The exposure lamp has a official name: Oriel Flood Exposure Source, unit 92540. All other parts of equipment: substrate and mask holder with media tank, exhaust box around the tool, timer controller, were designed and build at DTU Danchip workshop.
The substrate and mask holder with a media tank was designed as part of Master Thesis of DTU Nanotech, Andres Kristensen group. The exhaust box was made as part of safety and the timer controller was build to control exposure time.
The technical specification and the general outline of the equipment can be found in LabManager.
The user manual(s), quality control procedure(s) and results and contact information can be found in LabManager.
| Purpose |
UV exposure | ||
|---|---|---|---|
| Performance | Exposure mode |
| |
| Exposure light/filters |
| ||
| Minimum structure size | |||
| Mask size |
5x5inch optinal | ||
| Alignment modes |
No alignment possible | ||
| Substrates | Substrate size |
Up to 8inch substrates, different shapes | |
| Allowed materials |
All cleanroom materials | ||
| Batch |
1 | ||