Jump to content

Specific Process Knowledge/Thin film deposition/Deposition of Silicon Oxide/Deposition of Silicon Oxide using PECVD: Difference between revisions

From LabAdviser
Bghe (talk | contribs)
No edit summary
Bghe (talk | contribs)
No edit summary
Line 2: Line 2:




At the moment DANCHIP has 2(3) PECVDs that can deposite silicon oxide with or without dopants of Boron, Phosphorous or Germanium. PECVD1 has been decommissioned and PECVD3 are for silicon based processing allowing wafers with small abount of metal (<5% wafer coverage). PECVD2 is for clean wafers both for silicon based materials and for III-V materials. At the moment PECVD2 is described under III-V processing. Look at the [[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]] page to learn more about the PECVDs at DANCHIP. All though PECVD2 and PECVD3 are very much alike you cannot count on the a recipe on one system will give exactly the same results on the other system.
At the moment DANCHIP has 2(3) PECVDs that can deposite silicon oxide with or without dopants of Boron, Phosphorous or Germanium. PECVD1 has been decommissioned and PECVD3 are for silicon based processing allowing wafers with small abount of metal (<5% wafer coverage). PECVD2 is for clean wafers both for silicon based materials and for III-V materials. Look at the [[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]] page to learn more about the PECVDs at DANCHIP. All though PECVD2 and PECVD3 are very much alike you cannot count on that a recipe on one system will give exactly the same results on the other system.


=Recipes on PECVD2 for deposition of silicon oxides=
=Recipes on PECVD2 for deposition of silicon oxides=

Revision as of 15:28, 15 July 2014

Feedback to this page: click here


At the moment DANCHIP has 2(3) PECVDs that can deposite silicon oxide with or without dopants of Boron, Phosphorous or Germanium. PECVD1 has been decommissioned and PECVD3 are for silicon based processing allowing wafers with small abount of metal (<5% wafer coverage). PECVD2 is for clean wafers both for silicon based materials and for III-V materials. Look at the PECVD page to learn more about the PECVDs at DANCHIP. All though PECVD2 and PECVD3 are very much alike you cannot count on that a recipe on one system will give exactly the same results on the other system.

Recipes on PECVD2 for deposition of silicon oxides

Quality control recipe

Quality Controle (QC) for PECVD2
QC Recipe: QCTOXIDE
SiH4 flow 12 sccm
N2O flow 710 sccm
N2 flow 392 sccm
Pressure 550 mTorr
RF-power 100 W @380kHz
Deposition time 1 min
QC limits PECVD2
Depostion rate of Silicon Oxide 69nm/min - 119nm/min
Non-uniformity of the deposition rate (std. deviation of 9 points) 0 - 2.8 nm
Refractive index of the Silicon Oxide 1.41 - 1.53
Non-uniformity of the refrative index (std. deviation of 9 points) 0 - 0.07

SiO2 Standard, High Rate

SiO2 Standard
N2O-flow 1600 sccm
SiH4-flow 17 sccm
RF-power (380 kHz) 380 W
Process Pressure 400 mTorr
Deposition rate 179 nm/min
index of refraction 1.461

SiO2 Standard, Low Rate

1STOxide A test recipe
N2-flow 392 sccm 392 sccm
N2O-flow 1420 sccm (setting in software is 710 sccm) 1420 sccm (setting in software is 710 sccm)
SiH4-flow 12 sccm 12 sccm
RF-power 100 W 150 W
Process Pressure 550 mTorr 700 mTorr
Deposition rate ~100 nm/min 109 ± 2 nm/min [tested: 2014-03-18]
index of refraction 1.47 1.465 [tested: 2014-03-18]
Uniformity <1 % 3.2% over the wafer [tested: 2014-03-18]


Deposition rate as a function of deposition time using 1STOxide:

Deposition time [s]

Oxide thickness [nm] Expected naturally grown oxide [nm] Deposition rate [nm/min]
15 26.9 2 99.6
30 51.9 2 99.8
60 102.4 2 100.4
60 102.7 2 100.7
120 201.1 2 99.6


Thickness uniformity of test wafer using the test recipe

Thickness uniformity of test wafer using the test recipe.


Recipes on PECVD3 for deposition of silicon oxides

Quality Controle (QC) for PECVD3 - oxide
QC Recipe: QCOXYD
SiH4 flow 12 sccm
N2O flow 1420 sccm
N2 flow 392 sccm
Pressure 550 mTorr
RF-power 60 W
QC limits PECVD3 - OXIDE
Deposition rate 66 - 89 nm/min
Non-uniformity <1.9%
Refractive index 1.472 - 1.487

Recipes

Recipe name SiH4 flow [sccm] N2O flow [sccm] N2 flow [sccm] B2H6 flow [sccm] PH3 flow [sccm] Pressure [mTorr] Power [W] Description
LFSiO 12 1420 392 0 0 550 60 Uniform silicon oxide
1PBSG 17 1600 0 135 40 500 800LF BPSG glass for waveguide cladding layer

LF=Low Frequency

Expected results

Recipe name Deposition rate [nm/min] RI Uniformity [%]
LFSiO ~75 ~1.48 <1
1PBSG ~228 nm/min . ~17%

Recipes on PECVD3 for deposition of doped oxide

Recipes

Recipe name SiH4 flow [sccm] N2O flow [sccm] N2 flow [sccm] GeH4 flow [sccm] (scaled by 100) B2H6 flow [sccm] PH3 flow [sccm] Pressure [mTorr] Power [W] Description
Core-Ge 17 1600 300 300 0 0 400 600 LF Process for germanium doped core layer developed by Haiyan Ou from DTU Photonics

Annnealing: Anneal bond furnace, recipe "core1100"

Top-BPSG 17 1600 0 0 100 40 500 800 LF Process for PBSG top clading layer developed by Haiyan Ou from DTU Photonics

Annnealing/oxidation: Anneal bond furnace, recipe "clad1000"

Expected results

Recipe name Deposition rate [nm/min] Refractive index
Core-Ge ~188 nm/min ~1.46969
Top-BPSG ~248 nm/min ~1.458


Recipes on PECVD1 for deposition of silicon oxides Expired!

Recipes

Recipe name SiH4 flow [sccm] N2O flow [sccm] N2 flow [sccm] B2H6 flow [sccm] PH3 flow [sccm] GeH4*100 flow [sccm] Pressure [mTorr] Power [W] Description
1oxide/1ox_std/standard 17 1600 0 0 0 0 400 380LF Process control recipe. Developed for waveguides
1PBSG 17 1600 0 135 40 0 500 800LF Developed for waveguide top cladding by Haiyan Ou @DTU Photonics'.
BGE_PBSG 17 1600 0 240 60 0 500 800LF Low stress PBSG
HO_core 17 1600 300 0 0 400 400 600LF Developed by Haiyan Ou @fotonik@dtu
HO_top 17 1600 0 107 40 0 500 800LF Developed by Haiyan Ou @fotonik@dtu

Expected results

Recipe name Deposition rate [µm/min] RI Uniformity [%] Comments
1oxide/1ox_std/standard ~0.193 1.46 2 The latest measured values can be seen in the process control sheet in LabManager
1PBSG ~0.3 1.458@633nm